Research Progress on Molecular Reaction Mechanisms and Design of Vacuum Residue Hydrotreating Catalysts

Submitted:

23 November 2026

Posted:

25 November 2026

You are already at the latest version

Abstract
Asphaltenes and metalloporphyrins in vacuum residue are large and prone to aggregation; consequently, their hydroconversion is constrained by both active-site reactivity and intraparticle mass transfer, while catalyst development has traditionally relied on empirical correlations. Based on the concept of molecular management in petroleum refining, this review examines the molecular-scale principles underlying the design of residue hydrotreating catalysts. Estimates based on the Yen–Mullins model and the Renkin equation indicate that when the pore diameter is approximately 9–10 times the diameter of the diffusing unit, the effective intrapore diffusivity can remain above 60% of its bulk value (approximately 18–20 nm for nanoaggregates and 44–50 nm for clusters). However, this criterion is sensitive to aggregate size and should be regarded only as an order-of-magnitude guideline. Density functional theory (DFT) calculations and scanning tunneling microscopy studies indicate that brim sites and sulfur vacancies at the edges of Ni(Co)MoS govern the hydrogenation (HYD) and direct desulfurization (DDS) pathways, respectively. Metalloporphyrins undergo demetallization through hydrogenation followed by ring opening, whereas competitive adsorption by basic nitrogen compounds and dehydrogenative condensation of aromatic cores are the molecular origins of nitrogen inhibition and coke formation, respectively. The relative advantages of Type I and Type II active sites vary with temperature and the rate-limiting step. The resulting relationships among key molecules, reaction characteristics, and design strategies provide a basis for the rational design of active phases, hierarchical supports, and catalyst grading.
Keywords: 
;  ;  ;  ;  
In 2024, China’s crude oil processing volume exceeded 7 × 10⁸ tonnes [1]. Against the backdrop of increasingly heavy crude oils and refinery restructuring, demand for low-sulfur marine fuel oil, low-sulfur petroleum coke, and high-quality fluid catalytic cracking feedstocks has increased the importance of vacuum residue hydrotreating [2,3]. Fixed-bed residue hydrotreating remains the predominant technology in China, and its long-term operation depends to a great extent on catalyst performance [4].
The challenges in designing residue hydrotreating catalysts originate from the nature of the feedstock. Asphaltenes and resins occur as nanoaggregates, within which Ni and V are incorporated mainly as porphyrin complexes. These molecules must diffuse into catalyst pores before reacting, while the resulting metal sulfides and coke deposit inside the pores and progressively block the pore entrances [4,5]. Conventional catalyst development has relied largely on empirical correlations between pore structure and performance, together with industrial testing. Advances in DFT calculations, atomic-resolution characterization, and molecular simulations now make it possible to explain these phenomena at the molecular and atomic levels.
Advances in high-resolution mass spectrometry have enabled molecular-level characterization of heavy oils. The heavy-oil research team at China University of Petroleum (Beijing) has conducted systematic studies involving supercritical fluid extraction and fractionation (SFEF), Fourier transform ion cyclotron resonance mass spectrometry (FT-ICR MS), and molecular reconstruction. These studies led to the concept of “molecular management,” which involves establishing reaction networks and kinetic models based on molecular composition to optimize processing operations [6]. Combined SFEF and mass-spectrometric analyses have shown that molecular weight and aromaticity increase with fraction heaviness, with most asphaltenes concentrated in the terminal fraction [7]. Molecular reconstruction provides a method for representing the molecular composition of residues [8]. These studies reveal the molecular identities of the reactants; catalyst design must additionally establish which molecules approach active sites and the sizes and structures with which they do so.
Nevertheless, a substantial gap remains between understanding molecular composition and designing catalysts. Existing reviews have focused mainly on process developments or catalyst composition [2,9], whereas DFT and scanning tunneling microscopy (STM) studies of active phases have generally used small probe molecules such as thiophene and dibenzothiophene. The two areas have not been adequately connected; consequently, key questions such as the appropriate pore diameter and the optimal active-phase structure are still answered largely through empirical experience.
To address these issues, this review is organized around the relationship “key molecules–reaction characteristics–design strategies.” First, the key reactants governing catalyst performance and the characteristics of catalyst deactivation are identified. The molecular mechanisms of hindered diffusion, active-phase structure, porphyrin demetallization, nitrogen inhibition, and coke formation are then discussed, with sensitivity and uncertainty analyses used to define the scope of the conclusions. On this basis, active phases, supports, and preparation methods are examined, followed by conclusions and perspectives.

1. Reaction Characteristics of Residue Hydrotreating and Industrial Catalyst Deactivation Patterns

1.1. Performance of Industrial Units and Characteristics of Spent Catalysts

Table 1 summarizes the operating indicators of representative fixed-bed residue hydrotreating technologies used in China and elsewhere [2]. Most technologies achieve metal-removal and sulfur-removal rates of 80–95%, whereas nitrogen removal and Conradson carbon residue (CCR) reduction are generally only 40–70%. This indicates that the conversion of nitrogen-containing polycyclic compounds and coke precursors remains a major limitation of current catalysts.
Spent industrial catalysts record the deactivation history under actual operating conditions. Pu et al. [5] analyzed a unit comprising five reactors in series and found that Ni and V deposition first increased and then decreased along the flow direction, with most deposition occurring on the demetallization catalysts in reactors 1–3. On R1-HDM3, Ni and V deposition reached 31.3% and 92.2%, respectively, relative to the fresh catalyst, whereas Fe and Ca were retained mainly by the guard catalyst (Figure 1). Within catalyst pellets, Ni was distributed relatively uniformly in the radial direction, while V and Fe were enriched near the outer rim [10,11]. Even after toluene extraction, the spent catalysts exhibited a mass loss of nearly 20%. Moreover, the combustion temperature of deposited coke increased along the flow direction, indicating a gradual transformation from soft coke to hard coke [12]. Accumulation of metal sulfides at pore mouths and coke deposition are the main causes of catalyst deactivation [4,5]; their molecular origins are discussed in Section 2.

1.2. Molecular Composition of Residue and Key Reactants

The challenges of residue hydrotreating can ultimately be traced to its molecular composition. Zhang et al. [7] separated Orinoco vacuum residue by SFEF into 13 extractable fractions and one terminal fraction. Electrospray ionization (ESI) FT-ICR MS analysis showed that the molecules were separated according to aromaticity and molecular weight, with most asphaltenes concentrated in the terminal fraction. Vapor-pressure osmometry (VPO), combined with the hindered stepwise association (HSA) model, showed that the initial association constant K1 depends on the number of aromatic rings, whereas the association hindrance factor H depends on aromatic-ring size and side-chain length [14]. Thus, the tendency to aggregate can be quantitatively related to molecular structure. Xu et al. [15] systematically characterized narrow fractions of Canadian oil-sands vacuum residue and its thermally cracked products and proposed representative molecular models.
The molecular forms of metal-containing components are similarly complex. Zhao et al. [16] identified several new series of vanadium compounds in Orinoco heavy crude oil. Some may contain additional aromatic rings, thiophene groups, and amino groups attached to the porphyrin framework, indicating that vanadium porphyrins are structurally much more diverse than previously recognized. Liu et al. [17] sequentially extracted vacuum residue using methanol, dimethylformamide (DMF), and toluene. The three extracts contained 9.04%, 22.19%, and 62.58% of the total vanadium, respectively. Vanadium in the toluene extract was the most difficult to remove and was presumed to occur as vanadium porphyrins bearing complex substituents. On this basis, the authors proposed that hydrodemetallization (HDM) catalysts should combine high hydrogenation activity with a large-pore structure [17]. This finding directly links the molecular form of vanadium to pore structure and hydrogenation functionality.
The conversion of sulfur- and nitrogen-containing molecules follows a similar trend: the greater the degree of condensation, the more difficult the conversion. Zhao et al. [18] elucidated the molecular structures and distributions of refractory polycyclic aromatic sulfur heterocycles during residue hydrotreating. Orbitrap mass-spectrometric analysis by Wang et al. [19] showed that highly condensed nitrogen- and sulfur-containing aromatics are difficult to convert because of steric hindrance, whereas aromatics containing more than four rings exhibit relatively high hydrogenation and saturation reactivity. Lu et al. [20] found that increasing catalyst concentration can significantly enhance aromatic-ring saturation in highly condensed compounds. Although these findings were obtained in slurry-bed systems, they suggest that the conversion of sterically hindered, large heteroatom-containing molecules depends more strongly on hydrogenation sites (Table 2).

2. Molecular-Level Reaction Mechanisms and Theoretical Calculations

2.1. Structural Characteristics of Heavy Residue Molecules and Hindered Intrapore Diffusion

According to the Yen–Mullins model, an asphaltene molecule consists primarily of an aromatic core containing approximately seven fused aromatic rings, with alkyl side chains attached; its characteristic size is about 1.5 nm. Several molecules form nanoaggregates of approximately 2 nm through π–π stacking, and these aggregates can further associate into clusters of approximately 5 nm [21]. Ni and V porphyrins are commonly enriched in the aggregates. Therefore, the “diffusing unit” passing through catalyst pores is, in many cases, an aggregate rather than an individual molecule.
It should be noted that the Yen–Mullins model provides characteristic sizes rather than fixed values [22]. The supramolecular assembly model proposed by Gray et al. [23] suggests that aggregation is also driven cooperatively by acid–base interactions, hydrogen bonding, and metal coordination, potentially producing porous network structures. The differences between the two models concern the effective aggregate size, compactness, and extent of dissociation at elevated temperatures. These parameters directly affect estimates of hindered diffusion. Moreover, the association constant varies with the number of aromatic rings and side-chain length [14], and aggregate size itself depends on the feedstock.
When the diameter of a diffusing molecule, dm, is comparable to the pore diameter, dp, intrapore diffusion is restricted by both steric hindrance and drag from the pore wall. The Renkin equation can be used for a semiquantitative estimate [24]:
Deff/D0 = (1-λ)2(1-2.104λ+2.09λ3-0.95λ5), λ = dm/dp
The calculated results (Figure 2) show that Deff/D0 is approximately 0.64 at λ = 0.1 and decreases to 0.38 at λ = 0.2. Accordingly, to maintain an effective diffusivity above 60% of the bulk value, pores should be 18–20 nm in diameter for nanoaggregates of approximately 2 nm and 44–50 nm for clusters of approximately 5 nm. This is consistent with empirical findings: the suitable pore diameter for Maya heavy-oil demetallization catalysts is 10–25 nm [9]. The PHR series of demetallization catalysts incorporates “diffusion pores” of approximately 2,300 nm, with pores larger than 100 nm accounting for more than 20% of the pore volume, thereby providing transport channels for cluster-sized components [25,26].
The above estimates are sensitive to the input dimensions (Table 3). Using Deff/D0 ≥ 0.6 as the criterion, diffusing units measuring 1.5–2.5 nm require pores of approximately 13–22 nm, whereas clusters measuring 5–6 nm require pores of approximately 44–53 nm. A change of 0.5 nm in the diameter of the diffusing unit changes the required pore diameter by approximately 4.4 nm. Increasing the criterion to 0.7 raises the required pore diameter by approximately 40%. In addition, the Renkin equation does not account for porosity, tortuosity, molecular nonsphericity, adsorption on pore walls, or pore-size distributions, and therefore generally overestimates the actual effective diffusivity in catalyst pellets. Conversely, partial dissociation of aggregates at reaction temperatures reduces their effective size. These two sources of deviation act in opposite directions. Thus, “a pore diameter approximately ten times the diameter of the diffusing unit” should be regarded as an order-of-magnitude criterion for distinguishing small mesopores from large mesopores. Its accuracy needs to be improved through molecular-dynamics simulations and direct measurements of intrapore diffusion.
Another consequence of diffusion limitation is the formation of a nonuniform metal-deposition profile (Figure 3). When the demetallization reaction is relatively fast compared with intraparticle diffusion (i.e., the Thiele modulus φ is large), metals are deposited mainly in the outer region of the pellet [10,11]. As a result, active sites near the center remain underutilized, while pore entrances become blocked prematurely (Figure 3a). Reducing the reaction rate in the outer region or shortening the diffusion path can move the deposition front inward and produce a more uniform distribution (Figure 3b). This provides a theoretical basis for designing nonuniform active-metal distributions and catalyst-pellet geometries.
Note: (a) Pellet cross-section and enlarged view of the pore-mouth region; the shaded outer shell represents the deposited layer, and λ = dm/dp. (b) Profiles are plotted according to the steady-state concentration distribution, cosh(φr)/cosh φ, for a flat plate with a first-order reaction (φ = 7.0, 2.6, and 0.6); the curves illustrate qualitative trends only.

2.2. Atomic Structure of Sulfide Active Phases and Reaction Pathways

The active phase of residue hydrotreating catalysts consists of Ni(Co)MoS nanosheets supported on γ-Al2O3. Promoter atoms are located at the edges of MoS2 slabs and significantly enhance intrinsic activity [27]. The edge sulfur coverage and the number of sulfur vacancies (coordinatively unsaturated sites, CUS) depend on the chemical potentials of H2 and H2S in the reaction atmosphere [28].
The discovery of brim sites is particularly relevant to residue hydrotreating. Using STM, Lauritsen et al. [29] observed a bright band with metallic electronic states (the “brim”) just inside the fully sulfided edge. Thiophene can adsorb and become hydrogenated at this site without requiring a sulfur vacancy. DFT calculations by Moses et al. [28] further demonstrated that the HYD pathway occurs mainly at brim sites, whereas the DDS pathway requires the formation of sulfur vacancies at the edge to enable C–S bond cleavage. For large residue molecules, sterically hindered alkyl-substituted dibenzothiophenes and fused-ring aromatics are unlikely to adsorb at vacancies through σ-bonding via sulfur atoms. They are more likely to adsorb with their aromatic rings lying flat on brim sites, followed by hydrogenation and then desulfurization. Metalloporphyrin removal likewise begins with hydrogenation (Section 2.3). Therefore, residue hydrotreating catalysts should prioritize sufficient edge length and hydrogenation capacity rather than simply maximizing the number of sulfur vacancies. Kibsgaard et al. [27] compared the promoting effects of Fe, Co, Ni, and Cu at the atomic scale, providing a basis for promoter selection (Figure 4).
Although Type II active phases generally exhibit higher intrinsic activity, they are not superior under all conditions or for every elementary step. Jiang et al. [30] prepared NiMo/γ-Al2O3 catalysts dominated by Type I or Type II sites by adjusting the pH of the impregnation solution and the post-treatment conditions (Table 4). The two site types were represented by Ni–Mo–SO and Ni–Mo–SS models, respectively, in which inner-layer sulfur was replaced by oxygen in the former model, whereas the latter was fully sulfided. DFT calculations showed that the H2 dissociation barrier was lower at Type I sites (72.53 vs. 125.07 kJ/mol), favoring hydrogenation and saturation of side-ring aromatics. At Type II sites, the C–N bond-cleavage barrier of the fully hydrogenated acridine intermediate (THA) was lower (157.74 vs. 186.90 kJ/mol), favoring hydrogenolysis. VGO hydrotreating experiments were consistent with these results: at 340 °C, the nitrogen content of the Cat-I product was approximately 68.4% of that of Cat-II, whereas the trend reversed at 370 °C (1.7 ± 0.3 vs. 5.3 ± 0.5 μg/g) [30].
Table 4 Comparison of the preparation, structure, and performance of NiMo/γ-Al2O3 catalysts dominated by Type I and Type II sites [30].
Notably, the barrier for the first hydrogenation of the side ring of acridine is actually higher at Type I sites (96.82 vs. 74.57 kJ/mol). The advantage of Type I sites arises from the lower barrier for the rate-limiting H2 dissociation step [30]. This indicates that which site type is more favorable for hydrogenation depends on the identity of the rate-limiting step. For fused-ring nitrogen compounds that undergo hydrogenation followed by hydrogenolysis, the two site types may favor different elementary steps. Active-phase optimization should therefore account for the operating-temperature window and the position within the catalyst bed, rather than simply maximizing slab stacking or sulfidation degree.

2.3. Molecular Mechanism of Hydrodemetallization of Metalloporphyrins

Ware and Wei [31] established a sequential mechanism for HDM using nickel etioporphyrin (Ni-EP) as a model compound (Figure 5). The C=C bonds in the peripheral pyrrole rings of the porphyrin are first hydrogenated reversibly, producing dihydroporphyrin (Ni-EPH2) and then tetrahydroporphyrin (Ni-EPH4) intermediates. Subsequently, C–N bonds undergo hydrogenolysis and the macrocycle opens, with the metal deposited in the form of a sulfide. Vanadyl porphyrins follow a similar pathway, but are generally more reactive than nickel porphyrins [32].
This mechanism has two direct implications. First, hydrogenation is the rate-controlling step in HDM, and demetallization activity is closely related to the number of accessible hydrogenation sites. Second, metals are deposited in situ; the regions where reaction proceeds most rapidly are therefore blocked first. The distribution of active sites consequently determines whether the metal-retention capacity can be fully utilized. At present, DFT studies of the complete “adsorption–hydrogenation–ring-opening” sequence of porphyrins at NiMoS edges remain very limited.
Porphyrins in actual residues do not exhibit uniform reactivity. Approximately 62.58% of the vanadium occurs in the toluene-extracted fraction, which is the most difficult fraction to demetallize [17]. These species may be subject simultaneously to intrinsic hydrogenation difficulty and diffusion limitations arising from their association with aggregates. Although this hypothesis requires direct verification, it is consistent with the conclusion that HDM catalysts need to combine hydrogenation functionality with large pores [17]. This indicates that pore structure and active-site distribution must be designed cooperatively. In addition, differences between Ni and V in reactivity and deposition location [10,11,32] mean that their capacities and distributions should be evaluated separately.

2.4. Inhibition by Basic Nitrogen Compounds and Coke Precursors

Basic nitrogen compounds in residues compete with sulfur-containing molecules for active sites. Using DFT-derived adsorption-energy descriptors, Rangarajan et al. [33] analyzed more than 20 sites on unpromoted and Ni- or Co-promoted MoS2. They found that acridine adsorbs more strongly than dibenzothiophene at almost all sites. The only exception is the Ni-promoted sulfur edge (S-edge), where desulfurization experiences the least nitrogen inhibition. This provides a molecular-level rationale for preferentially selecting NiMo systems for feeds with high nitrogen contents. Nitrogen-containing heterocycles must be hydrogenated before their C–N bonds can be cleaved; therefore, hydrodenitrogenation (HDN) depends strongly on hydrogenation functionality. Calculations by Yin et al. [34] also showed that surface sulfur changes the HDN pathway of quinoline on MoP(010), indicating that the H2S atmosphere should be considered when evaluating new active phases such as phosphides.
Adsorption strength is also strongly site-dependent. Jiang et al. [30] calculated that acridine adsorption through coordination of its nitrogen atom to Mo is approximately 25–28 kJ/mol stronger than coordination to Ni; substitution of inner-layer sulfur by oxygen further strengthens adsorption. Therefore, the conclusion that “Ni weakens nitrogen inhibition” should be restricted to specific sites, such as Ni-modified S-edges. Meanwhile, the difficulty in converting highly condensed nitrogen-containing aromatics partly arises from steric hindrance [19]. Nitrogen inhibition thus involves both competitive adsorption and steric effects.
Coke mainly originates from the dehydrogenative condensation of fused-ring aromatics and asphaltene aromatic cores at acidic sites and high temperatures. The transformation of deposited coke from soft to hard coke on spent catalysts [12] is consistent with continued aromatic-core condensation and a decrease in the H/C ratio. Two approaches can suppress coke formation: (i) weaken strong acid sites on the support to reduce the initiation of condensation [9]; and (ii) enhance aromatic-ring hydrogenation to reduce stacking and association of aromatic cores. This also explains why catalysts in the front section of a reactor bed commonly combine weak acidity with high hydrogenation activity.
Figure 6 summarizes competitive adsorption by basic nitrogen compounds and the formation and suppression of coke, while Table 5 summarizes the molecular-level findings and their corresponding catalyst-design strategies.
Note: (a) Acridine is used as an example; thick solid lines indicate strong coordination, while dotted lines indicate weaker interactions [30,33]. (b) Dehydrogenative condensation of fused-ring aromatics at acid sites and strategies for its suppression [9,12]. Schematic illustration.

2.5. Multiscale Design from Molecules to Reactors

Multiscale design begins with the molecular composition of the feedstock. The molecular-management framework addresses three fundamental tasks: compositional characterization, molecular-composition modeling, and the construction and kinetic solution of reaction networks [6]. Figure 7 connects this framework to catalyst design. SFEF fractionation and high-resolution mass spectrometry provide molecular-composition data [7,15,16]. Molecular reconstruction is then used to assemble a molecular ensemble consistent with macroscopic properties [8]. Reaction networks for HYD, DDS, HDN, and HDM are subsequently established; their rate constants are determined experimentally and can be constrained using DFT descriptors. These networks are then linked to pellet-scale reaction–diffusion–deposition models and bed-scale deactivation models. The resulting outputs are mapped onto design variables, including pore-size distribution, active-site distribution, active-phase type, and catalyst-grading ratios, and are validated and refined using metal-deposition data from spent catalysts.
This workflow still has important limitations when applied to residues. The resolving power of mass spectrometry for heavy fractions and its ability to distinguish isomers remain limited. Automated construction and solution of reaction models containing thousands of components are not yet mature [6]. Consequently, industrial process models still commonly use lumped representations; for example, Wang et al. [35] used a six-lump model to describe the conversion of resins and asphaltenes. Molecular-composition data from slurry-bed systems [19,20] may provide parameters for molecular-level kinetic modeling, but their transfer to fixed-bed systems requires caution.
The reliability of the multiscale workflow also depends on error propagation. According to the Arrhenius relationship, an energy-barrier error of 10 kJ/mol at 653 K can produce an approximately 6.3-fold difference in the rate constant. The H2 dissociation barriers at the two site types reported by Jiang et al. [30] differ by approximately 52.5 kJ/mol, substantially exceeding this scale; the resulting trend is therefore robust. By contrast, the barriers of two hydrogen-transfer pathways at Type II sites differ by only 2.9 kJ/mol, which is insufficient to establish a reliable ranking. DFT results should therefore be used to identify trends involving clearly different energy scales, whereas absolute rate constants should be calibrated experimentally.
The above findings span several length scales (Figure 8). DFT provides information on site structures and energy barriers; molecular simulations describe asphaltene association and diffusion in confined pores; pellet-scale models predict deposition profiles; and reactor-scale deactivation kinetics support optimization of catalyst grading and operating cycles. The current bottleneck is the connection between scales. Most DFT studies still use small molecules or simplified porphyrins as probes, which differ substantially from the complex molecules in actual residues. Using metal-deposition and coke data from spent catalysts [5,12] as validation benchmarks is a practical way to narrow this gap.

3. Catalyst Design Based on Molecular-Level Understanding

3.1. Active Phases and Active-Metal Distribution

Type I NiMoS generally consists of single-layer slabs strongly bonded to the support through Mo–O–Al linkages, making complete sulfidation difficult. Type II slabs exhibit a certain degree of stacking, interact more weakly with the support, and can be more fully sulfided; consequently, they have higher intrinsic activity [9]. Zhu et al. [36] found that increasing the surface hydroxyl content of Al2O3 weakened metal–support interactions and generated more Type II active phases, increasing the sulfur-removal rate, CCR-reduction rate, and residue-conversion rate by 10.33%, 8.94%, and 3.46%, respectively. The metal-removal rate increased by only 1.05%; without replicate data, the statistical significance of this change is difficult to assess. In light of Section 2.2, residue catalysts should have a moderate degree of slab stacking, forming Type II structures while retaining sufficient edge length for adsorption of large molecules.
The spatial distribution of active metals is also important. At the catalyst-bed scale, guard catalysts and demetallization catalysts contain relatively low metal loadings to avoid excessively rapid reactions in the outer regions. Desulfurization and CCR-reduction catalysts have higher metal loadings to provide deep hydrogenation capacity. At the pellet scale, PHR-series demetallization catalysts employ a nonuniform “high-inner, low-outer” metal loading profile. A 14-month industrial basket test showed that these catalysts had higher metal-retention capacity and more uniform deposition [25,26]. New active phases such as Ni2P/SiO2 exhibit higher HDS and HDN conversions (98% and 80%) than industrial NiMoS/Al2O3 (78% and 43%) [9]. However, their stability under high H2S partial pressure and extensive metal deposition remains to be verified.
Catalyst grading is a direct means of translating molecular-level understanding into reactor-bed design. Jiang et al. [30] compared four grading schemes in a VGO system (Table 6). The arrangement with Type I catalyst in the first reactor and Type II catalyst in the second produced the lowest nitrogen content (3.4 ± 0.3 μg/g), whereas the reverse arrangement gave the highest value (10.1 ± 0.7 μg/g). For every scheme, the difference from the optimum exceeded 3.5 times the combined uncertainty, making the ranking reliable. The forward Type I/Type II arrangement matches the axial temperature rise in an adiabatic reactor: Type I sites provide a hydrogenation advantage in the lower-temperature section, while Type II sites favor hydrogenolysis in the higher-temperature section. It also matches the conversion sequence of fused-ring nitrogen compounds, in which side rings are first saturated and C–N bonds are subsequently cleaved by hydrogenolysis [30]. This strategy warrants testing in residue systems, although the front-end demetallization catalyst must also provide metal-retention capacity and resistance to pore blockage; the VGO arrangement should not be adopted without modification.

3.2. Pore Structure and Surface Properties of Supports

For residue hydrotreating, pore diameter and pore volume often have a greater influence than specific surface area. Kohli et al. [37] used NiMo catalysts supported on SBA-15, activated carbon, and mesoporous Al2O3 to process vacuum residue. Their specific surface areas were 573, 447, and 276 m2/g, respectively, whereas the corresponding HDS conversions were 51%, 61%, and 70% (Figure 9). However, the dataset contains only three samples (regression-slope p ≈ 0.075), and the surface chemistries of the supports differ substantially. The contribution of pore diameter therefore cannot be isolated. These data should be regarded only as trend-level evidence that specific surface area is not the sole determining factor.
China has accumulated considerable industrial experience in developing hierarchical-pore supports. Cheng et al. [26] used a nonacidic binder to form alumina without acid peptization and introduced composite pore expansion, achieving a proportion of 16.4% for pores larger than 1,000 nm. Tan et al. [25] constructed a hierarchical “millimeter–micrometer–nanometer” pore system in guard catalysts. Three-dimensionally interconnected macroporous Al2O3 prepared by Sui et al. [38] also exhibited good HDM performance. Pellet geometry affects performance by shortening the diffusion path. Spherical NiMo/Al2O3 catalysts achieved substantially higher HDM and CCR-reduction rates (78.20% and 39.43%) than cylindrical catalysts (65.20% and 17.50%) [9]. At the same outer radius, the characteristic diffusion lengths of spherical and infinitely long cylindrical pellets are R/3 and R/2, respectively; thus, the Thiele modulus of the spherical pellet is approximately one-third lower, consistent with the observed trend.
Regarding surface properties, increasing hydroxyl content favors the formation of Type II active phases [36], whereas weakening strong acid sites can suppress coke formation [9]. TiO2 modification can improve the HDS activity of Al2O3-based catalysts, but insufficient pore diameter may reduce HDM activity. CeO2 can inhibit the formation of NiAl2O4 spinel. Carbon–alumina composite supports can weaken metal–support interactions and reduce coke deposition at pore mouths [9], while carbon-nanotube@Al2O3 supports improve the dispersion and sulfidation degree of CoMo active phases [39]. P and B promoters can increase sulfidation and preferentially adsorb nitrogen-containing compounds. However, a P mass fraction above 2% reduces specific surface area and pore volume [9]. Therefore, lower promoter loadings are preferable for front-end catalysts, whereas the loading can be increased moderately in downstream catalysts.

4. Catalyst Preparation Methods

Supports are generally prepared from pseudoboehmite through kneading, extrusion, drying, and calcination. Conventional peptizing acids can cause excessive disintegration of crystallites and produce small pores. The use of nonacidic binders to achieve acid-free forming can substantially increase pore volume and pore diameter [26]. Pore-expansion methods such as hydrothermal treatment can also modify surface hydroxyl content and acidity. However, pore expansion is generally achieved at the expense of mechanical strength, requiring a balance between pore structure and crush strength [40].
Active components are mainly introduced by incipient-wetness impregnation. Adding competitive adsorbates to the impregnation solution or using sequential impregnation can produce a “high-inner, low-outer” metal distribution [26]. Chelating agents such as citric acid and EDTA coordinate with Ni2+ and delay its sulfidation. This allows Ni to migrate to the edges after the MoS2 slabs have formed, thereby increasing the proportion of the NiMoS phase and suppressing NiAl2O4 formation [9]. Promoter type and sulfidation conditions also have substantial effects on active-phase structure [40].
Table 4 clearly illustrates how preparation conditions regulate active-phase type. Impregnation at high pH followed by calcination at 500 °C produces Type I sites with a relatively low degree of sulfidation, whereas impregnation at low pH followed only by drying at 150 °C produces Type II sites with a higher degree of sulfidation [30]. The impregnation-solution pH, heat-treatment temperature, and use of chelating agents or phosphorus promoters are therefore key variables for controlling active-phase type. However, the mechanical strength and storage and transport stability of uncalcined catalysts remain to be evaluated.
Chelation strategies can also be applied to spent-catalyst regeneration. Citric-acid treatment can convert insoluble Ni and Mo species in oxidatively regenerated NiMoP/Al2O3 into complexes, restoring catalytic activity after sulfidation [41]. Ahn et al. [42] evaluated the feasibility of remanufacturing residue desulfurization catalysts. Table 7 summarizes the main methods for support construction and catalyst preparation.

5. Conclusions and Perspectives

This review has examined the molecular-level principles underlying the design of vacuum residue hydrotreating catalysts. The main conclusions are as follows: (1) Asphaltene aggregates are the principal diffusing units for intrapore mass transfer. A pore diameter approximately 9–10 times the aggregate diameter can maintain an effective diffusivity above 60% of the bulk value, although this should be treated only as an order-of-magnitude criterion. (2) Brim sites and sulfur vacancies correspond primarily to the HYD and DDS pathways, respectively. The conversion of sterically hindered sulfur compounds and metalloporphyrins is initiated by hydrogenation; edge length and hydrogenation capacity are more important than simply maximizing the number of sulfur vacancies. (3) Basic nitrogen compounds adsorb more strongly than sulfur-containing molecules at most sites, while Ni-modified S-edges experience the least inhibition. Coke originates from dehydrogenative condensation of aromatic cores at acid sites. (4) The relative advantages of Type I and Type II sites vary with temperature and the rate-limiting step. Active-phase design should therefore be coordinated with the operating-temperature window and catalyst-bed position. These findings provide a molecular basis for design strategies involving moderately stacked Type II active phases, hierarchical-pore supports, “high-inner, low-outer” metal distributions, and weakly acidic supports.
Most of the above understanding is derived from model compounds, simplified active-phase models, and idealized reaction conditions; its applicability to actual residue systems remains to be verified. Future research should focus on the following areas:
(1) Theoretical calculations involving molecules representative of actual residues. Fused aromatic cores bearing alkyl side chains, intact porphyrins, and their aggregates should be investigated using ab initio molecular dynamics and chemical potentials representative of reaction atmospheres. These studies should elucidate adsorption, hydrogenation, and ring-opening mechanisms at NiMoS edges, as well as aggregate dissociation and diffusion in confined pores.
(2) Closed-loop validation integrating molecular characterization, multiscale models, and industrial data. High-resolution mass spectrometry should be used to characterize feedstocks, products from different catalyst-bed sections, and deposits on spent catalysts. Quantitative relationships should then be established between reactant molecular structures, pore structures, and active-phase types [6,19,20]. Multiscale models should be validated against spent-catalyst data, with uncertainties explicitly propagated across all scales.
(3) Evaluation under realistic operating conditions and life-cycle-oriented design. The stability of new active phases, Type I/Type II site-grading strategies [30], and the balance between pore structure and mechanical strength should be tested in residue systems. Because spent residue hydrotreating catalysts are classified as hazardous waste (HW50) and contain valuable metals such as Ni, Mo, and V [13,43], and because calcination affects metal leaching [44], regeneration and metal-recovery performance should be considered from the catalyst-design stage [41].

Acknowledgments

The authors acknowledge the funding support from the following projects: the Ili Prefecture Science and Technology Plan Project (YJC2025B11) and the “Golden Triangle” Green Chemical Technology Innovation Center Project (XJYY2024YJPT09).

Conflicts of Interest Statement

All authors claim that there is no conflict of interest

References

  1. Jiayi, W.A.N.G.; Lei, T.I.A.N.; Shujun, B.A.O.; et al. Global oil markets are tending to ease: China’s refined oil consumption and crude oil imports both decline—Review of domestic and international oil market developments in 2024 and outlook for 2025 [J]. Energy China 2025, 47(3), 24–30. [Google Scholar]
  2. Da, W.U.; Shujiao, J.I.A.N.G.; Qiang, W.E.I.; et al. Research progress on efficient utilization technologies for residue amid the energy transition [J]. Chem. Ind. Eng. Prog. 2024, 43(5), 2343–2353. [Google Scholar]
  3. Fixed-bed residue hydrotreating technology adapted to refinery transformation and development [J]. GUO Shengjun YU Chuanrui WANG Fulin;Pet. Refin. Eng. 2024, 54(12), 9–12.
  4. Zhonghuo, D.E.N.G.; Lishun, D.A.I.; Rong, S.H.I.; et al. Progress and perspectives on the long-term operation of fixed-bed residue hydrotreating units [J]. Pet. Process. Petrochem. 2024, 55(9), 158–170. [Google Scholar]
  5. Ning, P.U.; Liang, R.E.N.; Qinghe, Y.A.N.G.; et al. Analysis of catalysts from an industrial fixed-bed residue hydrotreating unit after long-term operation [J]. Pet. Process. Petrochem. 2024, 55(9), 8–12. [Google Scholar]
  6. Quan, S.H.I.; Linzhou, Z.H.A.N.G.; Suoqi, Z.H.A.O.; et al. Molecular management for petroleum refining: Concepts and theoretical foundations [J]. Pet. Sci. Bull. 2016, 1(2), 270–278. [Google Scholar]
  7. ZHANG, L.; XU, Z.; SHI, Q.; et al. Molecular characterization of polar heteroatom species in Venezuela Orinoco petroleum vacuum residue and its supercritical fluid extraction subfractions[J]. Energy Fuels 2012, 26(9), 5795–5803. [Google Scholar] [CrossRef]
  8. ZHANG, L.; HOU, Z.; HORTON, S. R.; et al. Molecular representation of petroleum vacuum resid[J]. Energy Fuels 2014, 28(3), 1736–1749. [Google Scholar] [CrossRef]
  9. MAJODINA, S.; POSWAYO, O.; DEMBAREMBA, T. O.; et al. Towards improvement of hydroprocessing catalysts - understanding the role of advanced mineral materials in hydroprocessing catalysts[J]. Miner. Mineral. Mater. 2023, 2, 13. [Google Scholar] [CrossRef]
  10. Yuxia, D.I.A.O.; Hui, Y.U.A.N.; Limei, Q.I.U.; et al. Characterization of metal species on deactivated residue hydrotreating catalysts from an industrial unit [J]. Pet. Process. Petrochem. 2019, 50(7), 7–12. [Google Scholar]
  11. Kun, C.A.O.; Cheng, Z.H.A.N.G.; Yueming, G.U.A.N.; et al. Deposition and distribution of impurities on spent catalysts from an industrial fixed-bed residue hydrotreating unit [J]. Pet. Refin. Eng. 2022, 52(12), 49–53. [Google Scholar]
  12. Ning, P.U.; Qinghe, Y.A.N.G.; Dawei, H.U.; et al. Characteristics of coke deposited on catalysts from a long-running industrial residue hydrotreating unit [J]. Pet. Process. Petrochem. 2025, 56(4), 86–91. [Google Scholar]
  13. Ning, P.U.; Shouye, C.U.I.; Yong, H.E.; et al. Progress in the recovery of valuable metals from spent residue hydrogenation catalysts [J/OL]. Acta Petrolei Sinica (Petroleum Processing Section). 2026. Available online: https://link.cnki.net/urlid/11.2129.TE.20260710.0938.002.
  14. ZHANG, L.; ZHAO, S.; XU, Z.; et al. Molecular weight and aggregation of heavy petroleum fractions measured by vapor pressure osmometry and a hindered stepwise aggregation model[J]. Energy Fuels 2014, 28(10), 6179–6187. [Google Scholar] [CrossRef]
  15. XU, Z.; VAN DEN BERG, F. G. A.; SUN, X.; et al. Detailed characterization of virgin heavy oil resid and its thermally cracked resid[J]. Energy Fuels 2014, 28(3), 1664–1673. [Google Scholar] [CrossRef]
  16. ZHAO, X.; SHI, Q.; GRAY, M. R.; et al. New vanadium compounds in Venezuela heavy crude oil detected by positive-ion electrospray ionization Fourier transform ion cyclotron resonance mass spectrometry[J]. Sci. Rep. 2014, 4, 5373. [Google Scholar] [CrossRef]
  17. LIU, T.; LU, J.; ZHAO, X.; et al. Distribution of vanadium compounds in petroleum vacuum residuum and their transformations in hydrodemetallization[J]. Energy Fuels 2015, 29(4), 2089–2096. [Google Scholar] [CrossRef]
  18. ZHAO, J.; DAI, L.; WANG, W.; et al. Unraveling the molecular-level structures and distribution of refractory sulfur compounds during residue hydrotreating process[J]. Fuel Process. Technol. 2021, 224, 107025. [Google Scholar] [CrossRef]
  19. WANG, Y.; LU, J.; ZHANG, X.; et al. Molecular transformation of heavy oil during slurry phase hydrocracking process: A comparison between thermal cracking and hydrocracking[J]. Fuel 2023, 351, 128981. [Google Scholar] [CrossRef]
  20. LU, J.; WANG, Y.; ZHOU, Z.; et al. Molecular transformation of heavy oil during slurry phase hydrocracking process: Influences of operational conditions[J]. Pet. Sci. 2025, 22(2), 884–893. [Google Scholar] [CrossRef]
  21. MULLINS, O. C. The modified Yen model[J]. Energy Fuels 2010, 24(4), 2179–2207. [Google Scholar] [CrossRef]
  22. MULLINS, O. C.; SABBAH, H.; EYSSAUTIER, J.; et al. Advances in asphaltene science and the Yen-Mullins model[J]. Energy Fuels 2012, 26(7), 3986–4003. [Google Scholar] [CrossRef]
  23. GRAY, M. R.; TYKWINSKI, R. R.; STRYKER, J. M.; et al. Supramolecular assembly model for aggregation of petroleum asphaltenes[J]. Energy Fuels 2011, 25(7), 3125–3134. [Google Scholar] [CrossRef]
  24. RENKIN, E. M. Filtration, diffusion, and molecular sieving through porous cellulose membranes[J]. J. General. Physiol. 1954, 38(2), 225–243. [Google Scholar]
  25. TAN, Qingfeng; NIE, Shixin; Tao, C.H.E.N.G.; et al. Development and industrial application of PHR-series fixed-bed residue hydrotreating catalysts [J]. Chem. Ind. Eng. Prog. 2018, 37(10), 3867–3872. [Google Scholar]
  26. Tao, C.H.E.N.G.; Yusheng, Z.H.A.O.; Qingfeng, T.A.N.; et al. Development of PHR-series fixed-bed residue hydrodemetallization catalysts [J]. Chem. Ind. Eng. Prog. 2016, 35(10), 3219–3225. [Google Scholar]
  27. KIBSGAARD, J.; TUXEN, A.; KNUDSEN, K. G.; et al. Comparative atomic-scale analysis of promotional effects by late 3d-transition metals in MoS2 hydrotreating catalysts[J]. J. Catal. 2010, 272(2), 195–203. [Google Scholar] [CrossRef]
  28. MOSES, P. G.; HINNEMANN, B.; TOPSØE, H.; et al. The hydrogenation and direct desulfurization reaction pathway in thiophene hydrodesulfurization over MoS2 catalysts at realistic conditions: A density functional study[J]. J. Catal. 2007, 248(2), 188–203. [Google Scholar] [CrossRef]
  29. LAURITSEN, J. V.; NYBERG, M.; NØRSKOV, J. K.; et al. Hydrodesulfurization reaction pathways on MoS2 nanoclusters revealed by scanning tunneling microscopy[J]. J. Catal. 2004, 224(1), 94–106. [Google Scholar] [CrossRef]
  30. JIANG, Q.; DING, S.; HOU, S.; et al. Grading schemes of VGO hydrotreating catalysts according to the classification of their active sites[J]. RSC Adv. 2026, 16, 27495–27503. [Google Scholar] [CrossRef]
  31. WARE, R. A.; WEI, J. Catalytic hydrodemetallation of nickel porphyrins: Ⅰ. Porphyrin structure and reactivity[J]. J. Catal. 1985, 93(1), 100–121. [Google Scholar] [CrossRef]
  32. AGRAWAL, R.; WEI, J. Hydrodemetalation of nickel and vanadium porphyrins. 1. Intrinsic kinetics[J]. Ind. Eng. Chem. Process Des. Dev. 1984, 23(3), 505–514. [Google Scholar] [CrossRef]
  33. RANGARAJAN, S.; MAVRIKAKIS, M. On the preferred active sites of promoted MoS2 for hydrodesulfurization with minimal organonitrogen inhibition[J]. ACS Catal. 2017, 7(1), 501–509. [Google Scholar] [CrossRef]
  34. YIN, L.; MA, J.; LING, L.; et al. Insight into the hydrodenitrogenation mechanism of quinoline on the MoP(010) surface with and without the effect of sulfur[J]. Mol. Catal. 2023, 538, 112970. [Google Scholar] [CrossRef]
  35. WANG, Y.; SHANG, D.; YUAN, X.; et al. Modeling and simulation of reaction and fractionation systems for the industrial residue hydrotreating process[J]. Processes 2020, 8(1), 32. [Google Scholar] [CrossRef]
  36. ZHU, Huihong; PAN, Yunxiang; Lu, L.I.U.; et al. Construction of hydrotreating catalysts for low-quality residue and the mechanism underlying improved catalytic performance [J]. Chem. Ind. Eng. Prog. 2025, 44(5), 3009–3016. [Google Scholar]
  37. KOHLI, K.; PRAJAPATI, R.; MAITY, S. K.; et al. Effect of silica, activated carbon, and alumina supports on NiMo catalysts for residue upgrading[J]. Energies 2020, 13(18), 4967. [Google Scholar] [CrossRef]
  38. SUI, B.; WANG, G.; YUAN, S.; et al. Macroporous Al2O3 with three-dimensionally interconnected structure: Catalytic performance of hydrodemetallization for residue oil[J]. J. Fuel Chem. Technol. 2021, 49, 1201–1207. [Google Scholar] [CrossRef]
  39. KAZAKOVA, M. A.; VATUTINA, Y. V.; SELYUTIN, A. G.; et al. Design of improved CoMo hydrotreating catalyst via engineering of carbon nanotubes@alumina composite support[J]. Appl. Catal. B Environ. 2023, 328, 122475. [Google Scholar] [CrossRef]
  40. Jia, W.A.N.G.; Chong, P.E.N.G.; Lei, T.A.N.G.; et al. Regulation of the active-phase structure of residue hydrotreating catalysts and its effect on catalytic performance [J]. Chem. Ind. Eng. Prog. 2023, 42(4), 1811–1821. [Google Scholar]
  41. KLIMOV, O. V.; NADEINA, K. A.; BUDUKVA, S. V.; et al. Investigation of the regeneration of NiMoP/Al2O3 hydrotreating catalysts[J]. Appl. Catal. A General. 2022, 630, 118447. [Google Scholar] [CrossRef]
  42. AHN, S. Y.; NA, W. J.; KIM, K. J.; et al. Feasibility assessment on remanufacturing of Ni–Mo/γ-Al2O3 catalyst for residue hydrodesulfurization[J]. Catalysts 2023, 13(4), 738. [Google Scholar] [CrossRef]
  43. Hui, Y.U.A.N.; Wei, W.A.N.; Sutian, M.A.; et al. Hazardous-waste characteristics of spent residue hydrotreating catalysts [J]. Acta Pet. Sin. (Petroleum Processing Section) 2023, 39(6), 1403–1411. [Google Scholar]
  44. BAI, Y.; PU, N.; YANG, Q. H.; et al. Influence of roasting on the structure and leaching behavior of spent residue hydrotreating catalysts[J]. New J. Chem. 2026, 50(1), 411–423. [Google Scholar] [CrossRef]
Figure 1. Ni and V deposition on representative spent catalysts from an industrial fixed-bed residue hydrotreating unit [5,13].
Figure 1. Ni and V deposition on representative spent catalysts from an industrial fixed-bed residue hydrotreating unit [5,13].
Preprints 245870 g001
Figure 2. Hindered diffusion factor of asphaltene structural units versus pore diameter calculated by the Renkin relation.
Figure 2. Hindered diffusion factor of asphaltene structural units versus pore diameter calculated by the Renkin relation.
Preprints 245870 g002
Figure 3. Schematic illustration of diffusion–reaction–deposition at the pellet scale and qualitative radial metal-deposition profiles.
Figure 3. Schematic illustration of diffusion–reaction–deposition at the pellet scale and qualitative radial metal-deposition profiles.
Preprints 245870 g003
Figure 4. Schematic illustration of edge sites in the Ni(Co)MoS active phase and the structures of Type I and Type II active phases.
Figure 4. Schematic illustration of edge sites in the Ni(Co)MoS active phase and the structures of Type I and Type II active phases.
Preprints 245870 g004
Figure 5. Schematic illustration of the sequential hydrodemetallization pathway of metalloporphyrins. Schematic of the sequential hydrodemetallization pathway of metalloporphyrins.
Figure 5. Schematic illustration of the sequential hydrodemetallization pathway of metalloporphyrins. Schematic of the sequential hydrodemetallization pathway of metalloporphyrins.
Preprints 245870 g005
Figure 6. Schematic illustration of competitive adsorption of basic nitrogen compounds at NiMoS edges and the formation and suppression of coke.
Figure 6. Schematic illustration of competitive adsorption of basic nitrogen compounds at NiMoS edges and the formation and suppression of coke.
Preprints 245870 g006
Figure 7. Schematic workflow for molecular management, from molecular-composition characterization to catalyst and grading design. Note: SFEF, supercritical fluid extraction and fractionation; HRMS, high-resolution mass spectrometry; CCR, Conradson carbon residue. Steps 4 and 5 represent the connections proposed in this review; the other steps are adapted from Shi et al. [6] and Zhang et al. [8].
Figure 7. Schematic workflow for molecular management, from molecular-composition characterization to catalyst and grading design. Note: SFEF, supercritical fluid extraction and fractionation; HRMS, high-resolution mass spectrometry; CCR, Conradson carbon residue. Steps 4 and 5 represent the connections proposed in this review; the other steps are adapted from Shi et al. [6] and Zhang et al. [8].
Preprints 245870 g007
Figure 8. Schematic illustration of the multiscale design framework for residue hydrotreating catalysts.
Figure 8. Schematic illustration of the multiscale design framework for residue hydrotreating catalysts.
Preprints 245870 g008
Figure 9. Specific surface area and vacuum-residue HDS conversion of NiMo catalysts supported on different materials.
Figure 9. Specific surface area and vacuum-residue HDS conversion of NiMo catalysts supported on different materials.
Preprints 245870 g009
Table 1. Comparison of operating indicators of representative fixed-bed residue hydrotreating technologies in China and elsewhere [2].
Table 1. Comparison of operating indicators of representative fixed-bed residue hydrotreating technologies in China and elsewhere [2].
Technology Representative company Temperature (°C) Pressure (MPa) LHSV (h⁻¹) Metal removal (%) Sulfur removal (%) Nitrogen removal (%) CCR reduction (%)
RDS/VRDS CLG 350–430 12–18 0.2–0.5 92.0 94.5 70.0 50.0–60.0
RCD Unionfining UOP 350–450 10–18 0.2–0.8 78.3 92.0 40 59.3
Residfining Exxon 350–420 13–16 0.2–0.8 72.5 81.6 60.0–70.0 56.5
S-RHT Sinopec 350–427 13–16 0.2–0.7 83.7 92.8 72.8 67.1
RHT Sinopec 350–420 13–18 0.2–0.7 92.4 92.1 58.8 62.7
Note: S-RHT denotes an integrated residue hydrotreating technology; RHT denotes residue hydrotreating technology.
Table 2. Representative molecular-level studies on the characterization and conversion of vacuum residue.
Table 2. Representative molecular-level studies on the characterization and conversion of vacuum residue.
Research subject and method Main findings Implications for catalyst design
SFEF fractions of Orinoco vacuum residue; ESI FT-ICR MS [7] Molecules are separated according to aromaticity and molecular weight; asphaltenes are enriched in the terminal fraction Asphaltenes are heterogeneous; pore channels should be designed in a size-graded manner
SFEF fractions; VPO and HSA model [14] K1 depends on the number of aromatic rings, whereas H depends on aromatic-ring size and side-chain length Aggregate size varies with feedstock
Narrow fractions of bitumen vacuum residue and its thermally cracked products [15] Compositions, properties, and representative molecular models of the fractions were reported Provides input for molecular reconstruction
Molecular reconstruction of vacuum residue [8] Molecular ensembles reconstructed from aromatic cores, bridges, and side-chain building blocks Provides a basis for selecting DFT model molecules
Orinoco heavy crude oil; positive-ion ESI FT-ICR MS [16] New series of vanadium compounds containing aromatic rings, thiophene, and amino groups were identified DFT models should not be limited to simple porphyrins
Stepwise extraction and HDM of vacuum residue [17] The toluene extract contains 62.58% of the vanadium and is the most difficult fraction to demetallize High hydrogenation activity and large pores are both required
Slurry-bed hydrocracking; Orbitrap MS [19,20] Highly condensed heteroatom-containing aromatics are difficult to convert because of steric hindrance; increasing catalyst concentration enhances aromatic saturation Hydrogenation functionality is a limiting factor (reference only)
Table 3. Pore diameters required to reach target hindered-diffusion factors for different diffusing units (calculated by the Renkin relation).
Table 3. Pore diameters required to reach target hindered-diffusion factors for different diffusing units (calculated by the Renkin relation).
Diffusing unit Effective diameter (nm) Pore diameter (nm), Deff/D0 ≥ 0.7 Pore diameter (nm), Deff/D0 ≥ 0.6 Pore diameter (nm), Deff/D0 ≥ 0.5 Deff/D0 in 20-nm pores
Asphaltene molecule 1.5 18.4 13.2 10.0 0.72
Nanoaggregate 2.0 24.5 17.6 13.3 0.64
Nanoaggregate 2.5 30.7 22.0 16.7 0.57
Cluster 5.0 61.4 44.0 33.4 0.28
Cluster 6.0 73.6 52.8 40.0 0.21
Note: Numerical solutions of the Renkin equation give λ values of 0.0815, 0.1137, and 0.1498 for Deff/D0 values of 0.7, 0.6, and 0.5, respectively. The calculation assumes diffusion of rigid spherical molecules in straight cylindrical pores and does not account for porosity or tortuosity.
Table 4. Preparation, structure and performance of Type Ⅰ- and Type Ⅱ-dominated NiMo/γ-Al₂O₃ catalysts.
Table 4. Preparation, structure and performance of Type Ⅰ- and Type Ⅱ-dominated NiMo/γ-Al₂O₃ catalysts.
Parameter Type I-dominated (Cat-I) Type II-dominated (Cat-II)
Impregnation solution and pH Ammonium molybdate + nickel nitrate + ammonia; pH 10–11 MoO3 + nickel citrate + phosphoric acid; pH 1–2
Drying and calcination 120 °C × 4 h; 500 °C × 4 h 150 °C × 6 h; not calcined
Average stacking number / slab length 1.4 / 5.5 nm 3.3 / 6.4 nm
Proportion of sulfided Mo4+ (%) 59.3 71.1
H2 dissociation activation energy (Mo–S pair, DFT) (kJ mol⁻¹) 72.53 125.07
C–N bond-cleavage activation energy of THA (DFT) (kJ mol⁻¹) 186.90 157.74
Nitrogen content in VGO product at 340 °C (μg g⁻¹) 78.9 ± 1.1 115.3 ± 1.3
Nitrogen content in VGO product at 370 °C (μg g⁻¹) 5.3 ± 0.5 1.7 ± 0.3
Note: DFT data are based on the Ni–Mo–SO (Type I) and Ni–Mo–SS (Type II) models, respectively. Nitrogen contents refer to samples collected at the outlet of the second reactor in a two-stage series configuration; ± denotes the uncertainty reported in the cited study.
Table 5. Molecular characteristics of key residue species and corresponding catalyst-design strategies.
Table 5. Molecular characteristics of key residue species and corresponding catalyst-design strategies.
Key molecule/process Molecular-level understanding Catalyst-design strategy
Asphaltene aggregates [21,24] Molecules: approximately 1.5 nm; aggregates: approximately 2 nm; clusters: approximately 5 nm. Diffusion is strongly hindered when λ > 0.1 Use mesopores of approximately 20 nm together with diffusion pores ranging from hundreds of nanometers to micrometers
Metalloporphyrins [31,32] Hydrogenation precedes ring opening; metals are deposited in situ Ensure accessibility of hydrogenation sites; use a “high-inner, low-outer” activity distribution to shift the deposition front
Sterically hindered sulfur compounds [28,29] Difficult to adsorb through σ-bonding at sulfur vacancies; they mainly follow the brim-site hydrogenation pathway Increase edge length and hydrogenation capacity; use moderately stacked Type II active phases
Basic nitrogen compounds [33] Adsorb more strongly than sulfur compounds at most sites; Ni-promoted S-edges experience the least inhibition Prefer NiMo systems for high-nitrogen feeds and increase Ni promotion at the edges
Coke precursors [9,12] Aromatic cores undergo dehydrogenative condensation at acid sites, with soft coke evolving into hard coke Weaken strong acid sites and enhance aromatic-ring hydrogenation
Table 6. VGO hydrotreating results of Type Ⅰ/Ⅱ catalyst grading schemes and their uncertainty analysis[30].
Table 6. VGO hydrotreating results of Type Ⅰ/Ⅱ catalyst grading schemes and their uncertainty analysis[30].
Grading scheme (Reactor 1 / Reactor 2) Nitrogen content (μg g⁻¹) Relative uncertainty (%) BMCI Difference from optimum / combined uncertainty
Type I / Type I 6.9 ± 0.4 5.8 26.4 7.0
Type II / Type II 4.7 ± 0.2 4.3 25.8 3.6
Type I / Type II 3.4 ± 0.3 8.8 24.1 — (optimum)
Type II / Type I 10.1 ± 0.7 6.9 28.8 8.8
Note: Data are taken from Table 17 of Jiang et al. [30] (VGO; Reactor 1 at 340 °C and Reactor 2 at 370 °C; nitrogen content measured in the effluent from Reactor 2). The final column was calculated in this review as the difference divided by √(σ₁² + σ₂²), assuming that ± denotes standard deviation.
Table 7. Support construction and preparation methods for residue hydrotreating catalysts.
Table 7. Support construction and preparation methods for residue hydrotreating catalysts.
Preparation method Mechanism Structural parameters and effects
Acid-free forming + composite pore expansion [26] Prevents excessive crystallite disintegration and constructs a bimodal pore structure Pores >1,000 nm account for 16.4%; pilot test: 5,500 h; expected lifetime: >8,000 h
Hierarchical pore construction [25] Stepwise interception across millimeter-, micrometer-, and nanometer-scale pores Nanopores are concentrated around 13 and 250 nm; pores >100 nm account for 35%
Surface hydroxyl regulation [36] Weakens metal–support interactions and promotes Type II active phases HDS increases by 10.33%; HDCCR by 8.94%; conversion by 3.46%
“High-inner, low-outer” impregnation [25,26] Reduces the reaction rate in the outer region and shifts the deposition front inward 14-month basket test: higher metal-retention capacity and more uniform deposition
Chelation-assisted regeneration [41] Forms citrate complexes and reconstructs the active phase Activity of regenerated NiMoP/Al2O3 is restored after sulfidation
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.
Copyright: This open access article is published under a Creative Commons CC BY 4.0 license, which permit the free download, distribution, and reuse, provided that the author and preprint are cited in any reuse.