Abstract
Catalytic methane pyrolysis forms no CO₂ directly and, by stoichiometry, makes 2.98 kg of solid carbon per kg of hydrogen; viability depends on removing the carbon, retaining the catalyst, selling the carbon and keeping it solid, because oxidizing all of it later would release 10.9 kg of CO₂ per kg of hydrogen, comparable to steam reforming. One acid wash of a 5 g sample retained 91–95% of the carbon with metal below the 50 ppm detection limit; carbon from bismuth-based melts carries 52–83 wt% metal unless salt-capped; gasification can restore catalyst activity, variably, but consumes the product. The longest reported operation exceeds 500 h cumulatively, in two moving-bed pilots. Published model estimates span $1.7–8.2 per kg of hydrogen without carbon sale and $0.8–4.1 with it (2023 USD); once-through catalyst make-up at the median laboratory carbon-to-catalyst ratio would add about $8.3. Reported emission intensities span 0–25 kg CO₂-eq per kg of hydrogen because boundaries, methane leakage, heat supply, and carbon credits differ; each 1% of upstream methane leakage adds at least 1.2 kg, and no assessment quantifies later oxidation of the carbon. We propose a design-for-harvest hypothesis map, a reporting checklist, data structures for machine learning, and emissions-accounting rules.
Keywords: 
;  ;  ;  ;  ;  ;  ;  ;  

1. Introduction: The Carbon Problem

Steam methane reforming (SMR) supplies most of the world’s hydrogen at a production cost of about $1–1.2 per kg at low gas prices, or $1–2 per kg as a typical total cost, and emits about 10 kg of CO₂ for every kilogram of hydrogen [1]. Global hydrogen demand grew by almost 3% in 2025 to surpass 100 Mt [2]. Other low-carbon routes are being developed, among them water electrolysis [2], the gasification of biomass and other carbonaceous feeds [3] and biological hydrogen production [4]. Methane pyrolysis offers a different trade [5]. The standard reaction enthalpy of CH₄ → C + 2H₂ is 74.8 kJ per mol of methane, or 37.4 kJ per mol of H₂, against about 41 kJ per mol of H₂ for steam reforming to CO₂, from standard enthalpies of formation [6]; per mole of methane, pyrolysis needs less reaction heat but produces half as much hydrogen, and the carbon leaves the reactor as a solid instead of as CO₂ [1]. These are reaction enthalpies, not the process energy per kilogram of delivered hydrogen, and no CO₂ is formed by the reaction itself; emissions from heating, upstream methane leakage, and the end use of the carbon remain (Section 9.3). The cost of that trade is mass: each kilogram of hydrogen comes with 2.98 kg of solid carbon, so if all of today’s hydrogen output were hypothetically made by complete methane pyrolysis, the stoichiometric co-product would be about 300 Mt of carbon a year, nearly twenty times the global carbon black market of about 16 Mt a year [7]. This is an upper bound for illustration, not a forecast: current hydrogen comes from several feedstocks, and hydrogen burned for heat or lost in purification would raise the methane and carbon per kilogram delivered.
The carbon is therefore not a by-product to be handled after the chemistry is solved. It decides whether the process works at all, in three ways.
  • It ends the catalyst’s life. Carbon that encapsulates the active metal deactivates it; carbon that grows as filaments can carry the metal away with it. Without a way to remove or release carbon during operation, “the system inherently consumes the catalyst it relies on” [1].
  • It has to leave the reactor. A process making three times more solid than gas by mass must move that solid continuously, without blocking outlets, fouling walls, or entraining melt or catalyst.
  • It sets the cost. Selling the carbon is a major lever on the cost of hydrogen from pyrolysis [8], but its price depends on its grade, and the grade depends on how it was removed and purified.
Industry has met these problems directly. Graphitic Energy (formerly C-Zero), a molten-media developer, has begun a scale-up collaboration with Technip Energies (Section 9); Monolith, operator of a commercial plasma pyrolysis plant, announced in 2025 that it would switch its feed from natural gas to carbon black oil, so its expansion will not make carbon from methane [9]; and Hazer has commissioned cold-flow fluidization tests to de-risk the scale-up of its iron-ore process (Section 9).
The literature has grown quickly but along separate lines. The database search for this review found 2,705 eligible records on catalytic methane decomposition and methane pyrolysis, 138 of them reviews or perspectives (Section 2.1). They cover the field as a whole [10,11,12,13,14], catalysts [1,15,16], catalyst regeneration [17], carbon catalysts [18], molten media [19,20,21,22,23], reactors and technologies [24,25], carbon products and markets [7,26,27], and economics [8]. Table 1 compares the reviews closest to the present one, those that treat carbon removal, catalyst regeneration, carbon products or costs, with this review; all reviews and perspectives found by the search are listed in Dataset S5.
Two recent perspectives come closest to the question asked here. Le et al. [1] argue that carbon removal must be “a core requirement, not afterthoughts” of catalyst design and give a catalyst make-up cost framework, supported by a qualitative benchmark that supported catalysts rarely exceed a carbon-to-catalyst mass ratio of one. Musa et al. [8] give the carbon price that brings pyrolysis hydrogen to cost parity, but for the system as a whole, not by removal route or carbon grade. Weber et al. [28] re-evaluate literature data on nickel particle size, stability, and carbon properties, and Ba-Tuq et al. [29] tabulate catalyst, reactor, and cost indicators as reported. Carbon harvest as a design criterion, catalyst make-up cost, carbon markets, and cross-platform comparison therefore all have precedents. What has not been compiled from the primary studies is how often carbon recovery, product contamination, and catalyst fate are measured together, and what the measured values imply for catalyst make-up and hydrogen cost.
This critical review compiles evidence on solid-carbon recovery, product contamination and catalyst retention across methane-pyrolysis platforms, examines how often those outcomes are measured together, and identifies the measurements needed to connect laboratory carbon recovery to catalyst make-up and hydrogen-cost estimates. It is built on two datasets extracted from 185 published sources and checked against the source texts (Section 2.3 and Section 2.5): post-reaction carbon properties tied to the removal or regeneration route, and reactor and techno-economic data. Figure 1 sets out the chain the review follows, from catalyst design to carbon growth, removal, product grade and cost, and shows how rarely each link is reported. Section 3 treats catalyst design for harvest and what removal does to the catalyst; Section 4 compares removal and regeneration routes and sets out the few complete chains of evidence; Section 5 benchmarks continuous carbon withdrawal across reactor platforms; Section 6 resolves hydrogen cost by route and carbon grade and places measured carbon-to-catalyst ratios on the make-up cost framework; Section 7 audits machine-learning studies; Section 8 proposes a minimum reporting standard; and Section 9 sets out the industrial status, environmental boundaries and safety issues of scale-up. The aim is to tell catalyst, reactor, and process engineers what must be measured and achieved before methane pyrolysis can make hydrogen and carbon at scale.

2. Method and Dataset

2.1. Literature Search and Screening

This is a critical review supported by a structured evidence map; it is not a systematic review, but the search and selection are reported following PRISMA 2020 [30], adapted to an evidence map, and PRISMA-S [31] (Supplementary Figure S1 and Document S2). Two bibliographic databases were searched on 12 November 2026: Web of Science Core Collection and Scopus; the core query (Q01) without a year limit and the second query (Q02) for publication years 2010–2026. The core query (Q01) searched titles, abstracts, and keywords for methane pyrolysis, decomposition, cracking, thermolysis, splitting, or dissociation and for turquoise hydrogen. A second query (Q02) used proximity operators to find methane, CH₄, biogas, biomethane, or natural gas within four words of pyrolysis, decomposition, cracking, or thermolysis, combined with hydrogen or a solid-carbon term. Fourteen narrower queries on removal, regeneration, carbon products, reactors, costs, and machine learning (Q03–Q16) returned subsets of Q01 and served only to check coverage. The protocol strings, field tags, dates, filters and exported record files are given in Document S2; execution histories with per-line hit counts were not retained, so the numbers below are unique records exported per database, not database hit counts. Records were deduplicated by DOI, then by title and year, then by exact title with the same first author and a year within one. Earlier work and sources that the queries did not return came from an earlier full-text extraction round of this work, based on a broader bibliographic search, and from forward and backward citation searching; company releases, stock-exchange filings, conference papers, and trade press were added for the industrial status (other methods in Figure S1). The database search was run, and the datasets were closed on 12 November 2026; extraction from the first-round sources preceded it. The evidence cutoff is 12 November 2026 and includes articles available online by that date; six sources assigned to 2027 journal volumes were published online in 2026, as their DOIs indicate.
The exported files held 5,295 records from Web of Science (4,427 for Q01 over all years and 868 for Q02 only) and 5,450 from Scopus (4,445 and 1,005); removing 4,257 duplicates left 6,488 publications. The all-years run of Q01 also recovered 85 publications from 2010–2026 that an earlier, partial Web of Science export had missed. A phrase rule marked 2,020 records with no methane-decomposition process term in the title, abstract, or keywords as ineligible before screening. Random samples of these exclusions held one clearly eligible record in 60 and four possibly eligible records in 150 (Wilson 95% intervals 0.3–8.9% and 1.0–6.7%), suggesting that some tens of eligible records may have been lost at this step. A targeted re-screen of the 542 rule-excluded records at highest risk (nanotube or chemical-vapor-deposition terms together with methane, alternative-feed terms, or a missing abstract) found 11 eligible for the map (2.0%), mostly methane-fed nanotube syntheses; three carry harvest terms in their abstracts (a CO₂-regenerated chemical-looping carrier, a biogas-to-nanotube study reporting 63% purity, and a review of carbon catalysts). They are listed in Dataset S5 and were not extracted. Methane-fed vapor-deposition studies that use neither pyrolysis nor decomposition terms are therefore covered only in part. Screening then had two stages. Stage 1 asked only whether a record dealt with the decomposition of methane, natural gas or biogas into hydrogen and solid carbon. Of the 4,468 records screened on title and abstract, 1,763 were excluded, including retraction notices, corrigenda and one retracted article, and 2,705 were eligible for the evidence map; 104 borderline records were kept under an inclusive rule. Stage 2 asked whether a record carried harvest evidence: a removal, purification or regeneration step, the purity or residual metal of the carbon; an application test of the carbon; carbon withdrawal; catalyst or melt consumption; or a cost or life-cycle study that prices or places the carbon. The queries re-identified 169 eligible sources from the earlier extraction round; 15 more were added by other methods (the broader bibliographic search and citation searching of the earlier round, whose route is not recorded record by record), and four re-identified sources outside the scope of the map were kept as benchmarks or comparators and are shown separately in Figure S1. For these, Stage 2 used the full-text extraction: 51 carbon-dataset studies that reported none of the six harvest descriptors (49 re-identified, 2 from other methods) were moved to the map; they are cited where relevant but are not used in any figure or count. Of the 188 earlier-round sources, 117 remain in the two datasets, 51 were moved to the map, and the other 20 are the earlier-round papers of the machine-learning audit (10 re-identified, 7 from other methods and 3 comparators outside the map scope; Section 7); none was set aside as background or superseded. Conversely, one database record that the abstract tagging of Stage 2 had classed as map-only, a pilot study of two moving beds whose carbon withdrawal and run length are reported only in its full text [32], was added to the engineering and cost dataset. Extraction covers studies published from 2010 onward: the 101 earlier publications whose abstracts carry harvest terms are listed in Dataset S5 but were not extracted, and earlier work enters the datasets only through the earlier extraction round. The cut-off follows the scope of the earlier round and the period in which residual-metal, Raman, and cost reporting became common; the all-years search therefore defines the evidence map, not the extraction coverage. For the remaining records, 300 abstracts carried harvest terms. A strict re-screen kept 82 that report such evidence rather than mention it, 46 as background, and 172 in the map only. Full text was obtained for 69 of the 82, and these were extracted; the other 13 are not cited and contribute no values. In all, 185 unique sources entered the two datasets (102 in the carbon dataset and 101 in the engineering and cost dataset; 18 sources appear in both) and 23 papers the machine-learning audit (Section 7), for a total of 207 unique included sources (one machine-learning paper is also in the engineering and cost dataset); the remaining sources were used as background, industrial, or methodological sources. Screening, the strict re-screening, and full-text assessment were carried out under the authors’ direction with the help of SciSpace, as described in the declaration on generative AI and AI-assisted technologies. All values in this review come from published sources; medians, escalated costs, and make-up costs are secondary analyses of those values. The DOIs of the earlier-round sources were checked against Crossref, which corrected six identifiers; those of the new sources come from the database records and were matched against the full texts. No dataset source is retracted. One dataset source, an unpublished thesis abstract, was replaced by the peer-reviewed article of the same author [33]. Excluded, superseded, and background sources are distinguished in Supplementary Table S2, and every screening decision, with its reason, is listed in the search-audit workbook (Dataset S5). Sources outside the evidence map, such as thermodynamic data, policy and market documents, and related work on reforming, gasification, CO₂ capture, biochar and electrode materials, are cited for context only and enter no count.
A study entered the carbon dataset if methane, natural gas, or biogas was the carbon source and it reported at least one property of the carbon formed or of the spent catalyst. Purification studies on carbon from other feeds were kept as benchmarks but marked out of scope. Techno-economic, life-cycle and reactor studies entered the engineering and cost dataset if they reported a hydrogen cost, a carbon value, or a measured or modeled quantity of carbon withdrawal, catalyst or melt consumption, or run length. Both datasets keep the schemas of the earlier extraction round, so new and earlier studies are recorded in the same fields.

2.2. Data Extraction

Two structured schemas were written, piloted on 20 papers, and revised before full extraction (Supplementary Materials, Document S1).
  • Carbon dataset (Section 3 and Section 4). 102 sources, 283 catalyst or condition rows (273 of them from the 95 experimental, in-scope studies) and 50 fields: catalyst family, loading and support; reactor and conditions; carbon yield; growth mode and morphology; Raman, X-ray diffraction (XRD) and Brunauer–Emmett–Teller (BET) surface area of the carbon; residual metal and purity before and after removal; removal and regeneration route, sequence and conditions; regeneration cycles; and application tests. Of the 102 sources, 95 are experimental and in scope, 54 from the earlier extraction round and 41 from the database search; Figure 2 shows how often they report each post-reaction descriptor, and Supplementary Figure S2 shows the same data study by study. By the Stage 2 rule, every one of them reports at least one of the six descriptors needed to judge harvest, and 34 report three or more; the 51 earlier-round studies that reported none were moved to the map. All 185 dataset sources are listed in Supplementary Table S2, and every extracted value is given in the master data extract (Dataset S1).
Terms are used in fixed senses. Carbon purity means only a reported bulk or calculated carbon fraction. Residual metal (bulk, by ICP, XRF or digestion), ash (the TGA residue, which can include support and oxidized metal) and local EDS composition are recorded as separate descriptors and are not pooled. Atomic and mass percentages are not compared. For carbon flows, carbon formed is the carbon made by methane conversion; detached is carbon separated from the catalyst or melt; withdrawn is carbon removed from the reactor during operation; collected is carbon caught downstream, in a cyclone, filter, or skimmer; and recovered is carbon in the product stream as a fraction of the carbon formed, which needs a carbon balance. A share entrained to a cyclone or filter is reported as collected, not recovered, unless the source provides the carbon formed.
  • Engineering and cost dataset (Section 5 and Section 6). 101 sources giving 167 reactor rows (71 experimental, the rest simulations, models or values quoted in reviews), 161 techno-economic or life-cycle scenarios and 77 carbon-use rows. Reactor fields include platform, scale, run length, carbon-withdrawal method, fraction of carbon recovered, carry-over of metal or salt, catalyst or melt make-up, fouling, and particle growth. Cost fields include the levelized cost of hydrogen (LCOH) with and without carbon sale, the assumed carbon price and grade, break-even carbon prices, and catalyst or melt cost.
Rules were fixed before extraction. Removal means solid carbon was recovered; regeneration means carbon was gasified or burned off the catalyst. Carbon yields, purities, residual metal, and costs that exist only in figures were left blank rather than read off the plot; activity ratios after regeneration (Section 4.5), which several studies present only graphically, were read from the figures and are marked in Dataset S4. Carbon yields were recorded only when stated or obtainable by direct unit conversion, and never estimated from hydrogen formation. Inequalities and ranges were kept as reported. Costs were kept in the published currency and year.

2.3. Quality Control

A separate re-extraction of 45 randomly sampled cells from the carbon dataset, compared with the source texts, found 39 correct, 4 with minor discrepancies (rounding or basis not stated) and 2 wrong (4.4%; Wilson 95% confidence interval 1.2–14.8%, or 6.3–26.2% if the minor discrepancies are counted); all were corrected. These samples are meant to detect extraction problems, not to estimate the error rate of the whole dataset; the full quality-control reports are given in Supplementary Document S1. The errors concentrated in carbon yields, where 1 of the 8 sampled yield cells was wrong, so every plotted yield was rechecked. A check of 40 cells from the engineering and cost dataset found none wrong (95% upper bound 8.8%), and all 23 headline cost and engineering numbers matched their sources. The sample covers about 0.2% of the extracted cells, so the plotted values were checked separately. The 69 new full texts were extracted with the same schemas; for the first batch of 64, every numeric value in the 455 extracted fields was matched against the source text, and all 455 were found there, 7 after an explicit unit conversion, rounding, or decimal-comma reading. A further check of every value plotted in this review against the source text corrected three more entries: one metal loading, one carbon yield whose basis could not be confirmed, and Raman values measured after regeneration rather than on the as-produced carbon. Rows with physically implausible yields, data duplicated from another paper, or costs solved for a target rather than calculated are flagged and excluded from pooled statistics; the disposition of every flagged row is listed in Supplementary Table S3. Dataset S4 traces every plotted value to its study, page, table or figure, unit and basis. The authors then checked the data against the source publications in three steps. First, three authors checked by hand a stratified random sample of 30 plotted values and classes: all 24 numerical values were confirmed, four of them cost values after their currency and price-year conversion were recomputed, and two of six carbon-form classes were corrected; the correction was traced to the rule that assigns the classes, which was revised and reapplied, changing the class of 4 of 188 rows. Second, every value behind a conclusion was checked: each of the 96 values plotted in Figures 6, 10 and 11 and each of the 559 numbers quoted with a citation in the text and tables was searched for in the full text of its cited source, and 76 plotted values and 374 quoted numbers were found there with the same unit or were recomputed from numbers found there. Third, the same search was applied to a stratified random sample of 50 of the remaining plotted values (Figure 3, 7 and 9), of which 16 were found in the source text. Values that could not be matched automatically, mostly read from figures or from tables lost in text extraction, and the carbon-form classes are traced to their page, table, or figure in Dataset S4. The checklist with the outcome for every value is available from the corresponding author. In addition, the authors checked by hand every value quoted in the text, tables and figures against the full text of its cited source, including the values added during revision.

2.4. Normalization

Carbon yields are given per gram of fresh catalyst, including support and promoters but excluding inert bed diluent; values reported per gram of metal were converted only where the loading was stated, and values per gram of spent solids were not converted. Atomic-percent values of residual metal are kept as reported and excluded from weight-percent statistics. Costs were converted to 2023 US dollars using the US consumer price index (CPI-U, annual average) and, for euro values, the average exchange rate of the cost year. A general price index is used because the LCOH is dominated by feedstock and utility costs; escalating instead with the Chemical Engineering Plant Cost Index, as for plant equipment, changes no range limit by more than $0.6 per kg and does not change the order of routes (Supplementary Table S4, which also gives each original value, currency year, cost metric and assumption). Escalation places studies on one currency basis; it does not align their scales, prices, or boundaries. Where a study gives no currency year, publication year minus one is assumed and marked. Raman ratios are reported as published; laser wavelength and peak fitting differ between studies (20% of Raman rows state no wavelength, and the rest span 514–780 nm), so they are compared within studies. Cross-study medians are given only for 532 nm excitation.
The datasets, extraction records, extraction schemas, quality-control reports, and the machine-learning audit table are provided as Supplementary Materials.

2.5. Limitations of the Synthesis

The synthesis has four limits that readers should keep in mind. Studies differ in feed dilution, temperature, time on stream, and analytical method, so pooled medians describe the reported literature rather than intrinsic catalyst performance. Most carbon yields come from short batch runs. Costs from different studies rest on different scales, prices and boundaries, and are placed on one currency basis only to show their spread. The database search covers two databases; extraction covers studies from 2010 onward, so pre-2010 work enters the datasets only through the earlier extraction round; gray literature rests on citation searching, and 13 priority studies were available only as abstracts and contribute no values. Screening and extraction were not duplicated by a second independent reviewer, so inter-rater statistics such as Cohen’s kappa are not reported; accuracy was instead measured on random samples (Section 2.1 and Section 2.3). Stage 2 was also applied unevenly: earlier-round sources were judged on their full texts, but database records on title and abstract, and, apart from the one pilot study added from its full text and four map-only studies read in full to cite their catalyst findings (Section 3), which confirmed their classification, the remaining map-only records (1,997 eligible records without harvest terms in the abstract, excluding the 138 reviews and perspectives, and 172 kept in the map after the strict re-screen) were not checked in full text, so harvest evidence reported only in the body of a paper is under-represented among the 41 database-search studies relative to the 54 earlier-round studies. Finally, the frequency with which a quantity is reported reflects reporting practice; it does not indicate the prevalence of a mechanism or the success rate of a technology.
Additionally, since rows from one study are correlated, Figure 3 also presents the medians of study medians. Restricting the extraction to studies with harvest evidence narrows the base for catalyst-level statistics, such as carbon yield (Figure 3; Section 6.3), which therefore describe studies that bear on harvest rather than the catalyst literature at large. Adding back the 51 earlier-round studies without harvest descriptors would raise the median nickel yield from 1.7 to 4.9 g C per g catalyst (25 rows, 10 studies) and lower the once-through make-up cost of Section 6.3 from $8.3 to $6.5 per kg H₂ (37 studies, median ratio 2.3).

3. Design for Harvest: Catalyst Science

Catalyst studies in methane decomposition are usually judged by conversion, lifetime, and carbon yield. For a process that must recover carbon and keep its catalyst, three further outcomes matter: whether the carbon can be detached, whether the metal leaves with it, and whether the catalyst survives to be used again. This section reviews the catalyst literature for those outcomes.

3.1. Where Carbon Grows: Growth Mode and Metal–Support Interaction

In situ electron microscopy shows filamentous carbon nucleating at the step edges of nickel particles, with the particle carried to the fiber tip and reshaping as the fiber grows; the catalyst dies when graphene layers fully enclose the particle [54]. Whether the metal ends up at the tip or stays at the base depends on how strongly it is anchored. A weakly anchored particle lifts off the support and travels with the filament (tip growth); a strongly anchored one stays on the support while carbon grows away from it (base growth) [1,55].
The two modes have opposite consequences for harvest. Tip growth makes carbon easy to dislodge but takes the metal with it, so the product carries metal, and the catalyst is consumed [1]. Base growth keeps the metal on the support and may therefore allow the carbon to be sheared or sieved off and the catalyst returned. Kutteri et al. [36] found that Fe/SiO₂ gave base-grown nanotubes selectively and proposed it as easier to harvest with catalyst reuse, while Ni–Fe on the same support gave tip-grown fishbone fibers. The evidence for these statements is post-run microscopy of where the metal sits, so base growth remains a design hypothesis; it does not by itself show that the carbon detaches mechanically, that the product is low in metal, or that the catalyst can be reused. Those outcomes were measured together in only one solid-catalyst study, and for tip-grown tubes: ultrasonication and magnetic separation recovered 45–50% of the nanotubes with under 0.5% metal, and the recalcined catalyst returned to its initial activity, above 90% methane conversion, after each of five regenerations [56]. Figure 4 shows examples from the open-access literature of base and tip growth, of nickel particles encapsulated in carbon or carried at tube tips, and of carbon formed under a molten-salt cap.
Particle size acts through the same balance. On Ni/Al₂O₃, particles larger than about 20 nm formed nanotubes and lasted longer, while particles below 10 nm were encapsulated by graphitic layers and deactivated quickly [60]. On hydrotalcite-derived Ni catalysts, larger particles gave tip-grown, well-graphitized tubes and the deactivation factor rose linearly as particles became smaller [57]. Support chemistry can switch the outcome: Co–MgO calcined to a (Co, Mg)O solid solution gave only graphitic filaments, whereas reducible cobalt oxide phases gave shapeless tangles or encapsulating shells [61]. Anchoring must therefore be strong enough to hold the metal but not so strong that the metal cannot be reduced and stay active [1]. Support phase, promoters and loading act on the same balance. On Co–Rh/TiO₂, anatase-rich supports gave smaller multi-walled nanotubes with a narrower diameter distribution and better stability than rutile-rich ones, while amorphous supports favored CHₓ-type carbon [62]; in co-precipitated Ni–Co–Al catalysts, Zn kept the metal particles small and gave long, thin nanotubes over an 80 h test, whereas unpromoted catalysts sintered and grew wider tubes [63]; and on Co/TiO₂–Al₂O₃, stability rose with Co loading, with particles below 25 nm at 50 wt% [64]. These studies describe the carbon formed but report none of the six harvest descriptors (Section 2.1), so they remain in the evidence map rather than the harvest datasets. The same levers have long been tuned in the opposite direction in dry reforming and partial oxidation of methane, where carbon deposition is a main cause of deactivation [65,66,67,68]: the metal–support interface [69], metal dispersion on mesoporous silica [70], support porosity and phase, such as bimodal pores and mixed anatase–rutile phases [71,72], and promoters and second metals such as La, Ce, Fe, Mg and K [73,74,75]. A catalyst designed for carbon harvest needs the reverse outcome from these levers: carbon that grows away from a metal particle that stays anchored and active.

3.2. Carbon Capacity and Alloying

The carbon a catalyst can hold before it dies sets both the carbon-to-catalyst ratio of the spent solids and the purity of the product. Alloying is the main tool for raising it. Pd–Ni/SiO₂ accumulated at least 343 g C per g metal at 600 °C (converted from the reported molar ratio of a sample taken before deactivation) because the alloy particles did not form stable carbides and grew branched fibers, while Ni/SiO₂ deactivated through a nickel carbide [76]. Coprecipitated Ni–Cu–Al (10% Al) accumulated 585 g C per g Ni at 600 °C over 99 h [77], and Cu doping of fused Ni/Al₂O₃ roughly doubled accumulated carbon. It gave the purest product, 97.8 wt% C with 1.52 wt% metal [78]. The first two values are high partly because they are normalized to the mass of active metal, not to the fresh catalyst including support, and they are cumulative carbon inventories of single studies, not recoverable product yields; the make-up analysis in Section 6.3 uses carbon per gram of catalyst including support. Le et al. [1] attribute such gains to a second metal that changes carbon solubility and diffusion in the particle, delaying surface saturation; the explanations offered in the individual studies (carbide suppression, diffusivity) were inferred for those catalysts and conditions and have not been tested across systems. A third metal can trade the amount of carbon against its quality. Across a Taguchi design of hydrotalcite-derived Ni–Fe–Cu catalysts tested at 600 °C (7–21 wt% Ni, 0–4 wt% Fe, 0–2 wt% Cu), carbon yield ranged from 0.05 to 0.38 g C per g catalyst and was highest for 14 wt% Ni, 2 wt% Fe and 2 wt% Cu calcined at 700 °C, which grew fibers about 6 nm wide; Fe loading had the largest effect on performance and raised the disorder of the carbon (Raman ID/IG 1.3–2.1 across the series), Cu was associated with well-dispersed metal and less sintering, and the highest Ni loading gave thicker nanotubes of about 24 nm [79]. It reports none of the harvest descriptors either, so it also remains in the evidence map.
Across the dataset, the spread is wide (Figure 3b). Median yields across all rows are 1.7 g C per g catalyst for nickel (18 rows from 7 studies) and 0.8 for iron (15 rows, 6 studies); no other family is reported by three or more studies with harvest evidence. The order is not robust to the weighting: taking one median per study first yields 3.6 for nickel and 1.0 for iron, because a few studies contribute many rows. These values are the carbon formed by the end of each reported run, not the capacity of the catalyst. The runs lasted from 5 min to 100 h (median 2 h), mostly in batch and often on diluted methane, and longer runs reported more carbon (Spearman ρ = 0.58, 47 rows from 16 studies). Only two studies ran the catalyst to deactivation [43,49]; four report conversion falling, or carbon uptake approaching saturation, at the end of the run, one a catalyst still active, and nine do not report the state of the catalyst at the end in the text. Averaged over the run, the highest yield of each study corresponds to 0.1–14 g C per g catalyst per hour (median 0.7). Neither number is sufficient on its own: a rate describes productivity but not lifetime, and a cumulative yield from a run stopped early understates what the catalyst would hold. Low yields matter for harvest because they dilute the product: Co–Mo/Al₂O₃ at its optimum gave a product of only 38.8 wt% carbon, the rest being catalyst and support [80].
In the reported data, the form of the carbon follows the catalyst more closely than the reactor (Figure 3c). Of 188 rows from 73 studies that describe the carbon, iron gave nanotubes in 22 of 26 rows [37,39,41,52], nickel nanotubes in 15 [35,45,47] and fibers or filaments in 14 of 32 [49,81,82], molten metals graphitic flakes or sheets in 19 of 30 [38,53,59,83,84], molten salts mostly amorphous or pyrolytic carbon (9 of 16) [85,86,87], and plasma without a catalyst carbon-black-like spheres (5 of 7) [88,89]. Reactor and catalyst are confounded in these data: molten media were run almost only in bubble columns, and solid catalysts mostly in fixed beds, fluidized beds, or tube furnaces, so the two effects cannot be separated across families. Within one family, however, the form changes little with the reactor: iron gave nanotubes in fixed beds (13 of 16 rows) [37,41,50], fluidized beds (7 of 8) [39,44,90] and boats in tube furnaces (2 of 2) [91]. The form matters for harvest because it sets how the carbon holds the metal: nanotubes and fibers carry particles at their tips or bases (Section 3.1), graphitic flakes from melts trap melt, or salt between layers (Section 4.3), and disordered carbon is the first to be oxidized during purification [92]. These are frequencies of morphology labels in this corpus, with condition rows nested in studies, not rules: molten Cu–In droplets have given multiwalled nanotubes [34], and iron ore in an autothermal fluidized bed gave graphitic carbon [93]. The form reflects the evolving active phase (carbide, alloy or melt), its interaction with the support, the temperature, the gas composition and the carbon activity acting together, and most studies infer the growth route from microscopy rather than measure it. The classes are taken from the authors’ descriptions, which differ in detail and method, and a Raman ID/IG value alone does not measure nanotube purity, graphitization or performance.

3.3. The Operating Window

Operating conditions can keep a catalyst in the filament-forming regime. Zhang and Smith [94] defined a threshold ratio P(H₂)²/P(CH₄), measured at 500 °C on silica-supported cobalt and nickel and in that study’s pressure units, above which carbon forms as filaments with stable activity and below which it encapsulates the metal; the window widened with cobalt particle size, and the threshold is specific to the catalyst and temperature. Co-feeding hydrogen or raising its partial pressure lowers the carbon activity at the metal surface, at the cost of rate [1]. Temperature trades capacity for rate: on cobalt–alumina, raising the temperature from 475–500 °C to 600 °C raised conversion but cut catalyst life from 15–18.5 h to 3.5 h and carbon capacity from 60–63 to 34 g per g Co [95].

3.4. A Design-for-Harvest Map

Figure 5 combines these effects into a conceptual map of metal–support interaction against the form of carbon growth; it is adapted from the failure hierarchy of Le et al. [1], and its links are hypotheses to be tested, most of them not yet measured. Weak anchoring with filament growth results in detachable carbon but metal carry-over and catalyst loss, the first and most basic failure in the hierarchy of Le et al. [1]. Encapsulation, with weak or strong anchoring, deactivates the catalyst and leaves gasification as the only way to recover the metal, at the cost of the product. Strong anchoring with filament growth is proposed here as the most favorable case for supported catalysts, in which carbon might be removed mechanically and the catalyst returned. This is a hypothesis: anchoring strength is mostly inferred from where the metal sits in post-run micrographs rather than measured, and the carbon must still be separable from the support. Nor is it the only route, since tip-grown nanotubes have been recovered with under 0.5% metal by ultrasonication and magnetic separation while the catalyst was regenerated in batches [56]. In a fluidized bed of Ni/CeZrO₂, for example, the separated carbon fraction still held about 35 wt% catalyst and the spent catalyst kept 24–32% carbon after sieving and ultrasound [35].
The map is qualitative because data needed to place catalysts on it are often unreported. Growth mode is stated for only 40 of the 273 condition rows from experimental, in-scope studies, from 16 studies (tip 23, base 11, mixed 6), and only 8 rows report both growth mode and residual metal in the carbon. Design for harvest therefore needs two quantities reported together that are now reported apart: the growth mode, and the metal content of the carbon after the chosen removal step (Section 8).

3.5. What Removal does to the Catalyst

For a catalysis reader, removal has a second half: the state of the catalyst afterward. The four removal families act on it differently. Acid leaching dissolves exposed metal and oxide supports along with the impurities, so the catalyst is consumed and its metal must be recovered from the leachate if it is to be reused; one study in the dataset resynthesizes catalyst from the leachate, without reporting the fraction recovered [96]. Oxidative regeneration removes the carbon as CO or CO₂ and often, but not always, restores activity, and it can sinter or restructure the metal: Co–Fe/Al₂O₃ lost 44% of its surface area over eight oxygen-regeneration periods [58] (see also Section 4.5). Mechanical separation preserves the catalyst but recovers it with a few to tens of percent carbon still attached, and abrasion or handling losses of 5–15% of the catalyst mass per cycle have been measured [97]. In the molten-media runs reviewed, activity did not decline over up to 170 h, but melt is lost with the carbon, carbon can stay dispersed in or wet the melt, and salt is trapped in the product; these constraints depend on the system (Section 4.3 and Section 6.3). In the dataset, only 1 of the 35 regeneration studies reports the metal content after regeneration, and none reports metal lost per cycle, so the literature currently provides no measurable data on catalyst durability through repeated removal (Table 2).

4. Removal and Regeneration Routes

Two families of methods free a catalyst from its carbon, and they lead to different processes. Removal recovers the carbon as a solid product. Regeneration gasifies or burns it off; the carbon leaves as CO or CO₂ with oxygen, CO₂ or steam, or as methane with hydrogen, and the catalyst may or may not recover its activity. Mixed processes, in which part of the carbon is gasified and part is collected, are reported here by the fraction gasified, the solid collected, and the catalyst activity separately. Of the 95 experimental studies in the dataset, 56 report a removal or purification step and 35 a regeneration step (Figure 2). Few report what the step did to the carbon: 20 of the 56 removal studies give purity or residual metal after removal, and 5 give the fraction of carbon recovered; 5 of the 35 regeneration studies report Raman spectra after regeneration and 1 reports the residual metal after regeneration. Only one study reports a carbon mass balance through the step together with the purity of the product [51]; the acid wash of [96] reports the carbon retained from a fixed 5 g sample and its residual metal, not a process-level balance (Supplementary Figure S3).

4.1. Physical Removal from Solid Catalysts

Mechanical routes keep the catalyst intact and leave the carbon chemically unchanged, but they rarely recover most of it (Figure 6b). Sieving spent Fe/CaO-based catalysts on a 25 µm screen recovered about 10% of the deposited carbon as solid; the rest was steam-gasified to restore the catalyst [98]. Ultrasonication of spent Ni–Cu–Zn/Al₂O₃ in ethanol followed by magnetic separation of the catalyst recovered 45–50% of the nanotubes from solids containing 70 wt% carbon, but only 25–30% at 30 wt%, with under 0.5% metal in the recovered tubes [56]. In a Ni/CeZrO₂ fluidized bed, the separated carbon still held a third of its mass as catalyst (Section 3.4).
Separation works better when carbon is sheared off during operation. In a mechanocatalytic route, ball milling at 450 °C knocked carbon off single-atom-alloy milling balls as it formed and kept a Re/Ni catalyst active for 240 h. However, the carbon was collected only after the run [106]. Vigorous fluidization with 2.5% steam in argon removed nanotubes in situ from Fe/θ-Al₂O₃ at 850 °C, combining shear with selective gasification; 572 mg of tubes were collected over 10 cycles with about 86% carbon closure, though initial conversion fell from 90% to 40% [44]. Low-surface-area carbon spheres used as a support were designed to shed pyrolytic carbon by abrasion in a bubbling fluidized bed, and sieving then gave carbon with under 0.1 wt% residue [97]. These are the clearest demonstrations of design for harvest in a solid-catalyst system, and all three are at laboratory scale.
Three further mechanical variants show the same pattern. A swirling-flow device that tumbled spent reduced-ilmenite particles in a fast air stream knocked carbon off by attrition and carried it to a filter over ten decomposition–regeneration cycles, with 10% more hydrogen per gram of catalyst than a continuous 4 h run. However, the fraction of carbon recovered was not reported [107]. Vibratory separation of the carbon float layer from a 12 wt% Fe/Al₂O₃ fluidized bed gave a product of only 57 wt% carbon, because the nanotubes held 13.95 wt% Fe and 5.46 wt% Al, and four HCl washes still left more than 1 wt% of contaminants [90]. Segregation can enrich carbon at the top of a continuous fluidized bed. Still, a particle-scale model validated on a 3-inch column predicts that the carbon purity there falls from 72 to 39 wt% when the gas velocity doubles from 4.5 to 9.0 cm s⁻¹ [108]. Magnetic separation recovers the support or ore rather than the carbon: dense ZrO₂ beads coated with Fe₂O₃ were recovered and reused over three cycles once the iron–carbon product had been oxidized to magnetite [109], and a permanent magnet has been proposed to separate unspent magnetite ore from its carbon [110].

4.2. Chemical Purification

Acid leaching removes exposed metal and dissolves oxide supports (Figure 6a). For nanotubes grown from camphor and ferrocene rather than methane, included as a purification benchmark, concentrated HCl with 5 h of sonication raised purity from about 85% to over 98% and lowered ID/IG from 0.61 to 0.37 without wall damage, whereas sulfuric–nitric mixtures damaged and functionalized the tubes [111]. Time matters: boiling 5 M H₂SO₄ after pre-oxidation raised the nanotube content from 46.2% to 92.6% in 3 h, but a 6 h treatment began converting tubes to amorphous carbon [104]. Supports chosen to dissolve help: MgO-supported carbon purified to under 2.2 wt% residue in mild HCl [42], and removing an MgO-based Co–Mo catalyst raised powder conductivity from 55.5 to 67.6 S cm⁻¹ [112].
Acid cannot reach metal sealed inside carbon. Refluxing iron-ore-derived carbon in 12 M HNO₃ lowered iron from 15.2 wt% (19.6 wt% by thermogravimetric analysis, TGA) to 1.2 wt% by inductively coupled plasma (ICP) analysis, yet a TGA residue of about 7 wt% remained as encapsulated metal [100]. At the techno-economic end, a laboratory HNO₃ wash of a 5 g sample recovered 90.8–94.9% of the carbon with metal below the 50 ppm detection limit of the analysis, and the authors costed the route at scale [96]. The same chemistry serves catalysts used once through. HNO₃ reflux removed the residual catalyst from nanotubes grown on a hydrotalcite-derived iron catalyst (9.5 g C per g catalyst in 10 h) in place of regenerating it [50], and HCl or H₂O₂ washing of carbon from a molten Cu₀.₃₃Sn₀.₆₇ column lowered its metal content below 0.5 wt% [113]. Nanotubes grown at their base on a Cu-containing NiMo–Bi melt were skimmed off; a KCl layer and a dilute HCl wash raised the carbon to 96.87 wt% by XRF, with 0.77 wt% metal left and 95.7% of the mass recovered in washing, and the tubes served as a sodium-ion anode [51]. The reported purity depends on the method as much as on the treatment: purified iron-ore carbon showed 0.27 ppm iron by ICP after acid digestion but a TGA residue of 4.97 wt%, because encapsulated iron escapes the digestion [114,115]. Acid treatment adds reagent, waste, and a metal-recovery step, and its cost is reported separately in only one study (Section 6).

4.3. Molten Media: Carbon That Floats

Molten metals and salts make separation physical. Carbon is less dense than the melt and floats so that it can be skimmed or carried off with the gas. Molten Ni₀.₂₇Bi₀.₇₃ reached 95% conversion at 1065 °C with no deactivation over 170 h, and the carbon rose to the surface as graphitic powder [116]. Unwashed carbon from bismuth-based melts is heavily contaminated: carbon from Cu–Bi held 52.4 wt% metal [59], and carbon from Ni–Bi up to about 83 wt% [83]. A molten salt layer over the metal cuts the carbon sharply. A bromide cap over Ni–Bi lowered the metal in the carbon from about 83 wt% to under 5 wt% [83], and an NaCl layer over Cu–Bi lowered it to 2.2–3.8 wt%; washing and heating then gave up to 98.0 wt% carbon [59].
The salt itself then has to come out. After water washing, carbon from molten KCl contained 93.4 at% C, and after HCl washing 96.2 at% [86]. Ten hot-water washes left 2.3–3.3 at% Cl and some Mn and K in carbon from MnCl₂–KCl [117]. Solid-state nuclear magnetic resonance (NMR) shows why: salt is trapped inside the carbon and partly co-intercalated, so washing removes only surface ions [85]. In molten KCl alone, a large amount of carbon (more than 16 wt% of the salt) stayed dispersed in the melt or was entrained with it to the filter, and separation failed [118]. Pure tin is cleaner but less active; in a solar bubble column, 86–96% of the carbon was collected from the melt surface after the run [84]. The melt composition can also set the product and its purity: molten Cu–In at 1000 °C gave carbon fibers that, poured off the melt without washing, contained about 98.7 at% C with 0.9 at% In and 0.4 at% Cu by energy-dispersive X-ray analysis, and over 99.9% C after heat treatment at 1096 °C [119]; Cu–In droplets also gave multi-walled nanotubes [34]. Across molten-salt systems, carbon purity has so far reached about 98% [20]. In alkali-halide melts, water washing alone gave 55.0–91.6 wt% carbon, highest in NaCl, with purity following the wettability of the carbon by the salt [120], and a Ni–Bi layer under NaCl activated methane at the interface while the salt washed metal from the floating carbon [121].
Laboratory purities do not yet carry over to scale. The first multiscale characterization of carbon from a quasi-continuously operated molten-tin pilot reactor (crucible 150 mm × 1.5 m) found that the powder collected from the reactor and hot-gas filter contained 48.2 wt% carbon, was dominated by β-tin impurities, had a turbostratic structure without extended graphite stacking and a surface area of 11.9 m² g⁻¹ [122]. In a laboratory tin column, too, the floating carbon carried tin that EDS detected but that was not quantified [123]. Purification of pilot carbon, and its cost, remain to be shown.

4.4. Thermal and Electrochemical Purification

High-temperature treatment removes metal by evaporation and orders the carbon at the same time. Carbon from fluidized-bed decomposition on limonite ore, with 31.1 wt% ash, reached 99.82 wt% purity after 3 h at 2800 °C in vacuum, and its ID/IG fell from 0.73 to 0.29; an electrochemical anodic leach reached 99.59 wt% [101]. Annealing plasma carbon black at 1500 °C in argon raised its surface area from 36.5 to 172.7 m² g⁻¹ and its conductivity from 1.5 to 16.7 S cm⁻¹ [88]. Catalyst-free routes need a different clean-up. Plasma carbon carries no metal but adsorbed polycyclic aromatic hydrocarbons; solvent extraction removed them and raised the surface area from 57.9 to 80 m² g⁻¹ [124], and plasma carbon black annealed at 1000 °C reached 6.5 S cm⁻¹ and, as a conductive additive, a capacity close to that of a commercial carbon black [105]. Few-layer graphene from an arc plasma, collected by cyclone and bag filter, needed no purification at all [125]. These routes give the highest purities in the dataset, at energy costs that no study reports per tonne of carbon.

4.5. Regeneration by Gasification

Gasification rates of uncatalyzed carbon at 800 °C rank O₂ (relative rate about 10⁵) far above steam (3), CO₂ (1) and H₂ (3 × 10⁻³), although the order need not hold for catalyzed gasification [126]. The regeneration studies were done on different catalysts, at different temperatures and with different protocols, so the ranges below describe the reported cases and do not rank the agents. Activity is the conversion or rate each study reports, at the time in each cycle that it reports, and the ratio is last cycle over first. Across the dataset, oxygen or air regeneration gave 82–100% of the first-cycle activity over 3–8 cycles, CO₂ 42.9–81.3% over 5–10 cycles and steam 42–93% over 4–10 cycles (Figure 7; one point per catalyst; cycle counts, agents, temperatures and the plotted values are listed in Dataset S4). Oxygen burn-off at 850 °C fully restored Fe/TiO₂–Al₂O₃ over three cycles [41], but short in situ oxygen pulses on Co–Fe/Al₂O₃ left encapsulating carbon behind, and conversion fell from 68% to 56% over eight periods while surface area fell from 109 to 61 m² g⁻¹ [58]. Reverse-Boudouard regeneration with CO₂ gasified over 95% of the carbon each cycle on Ni [49], and adding FeOₓ to Ni/Al₂O₃ raised carbon removal from 89% to 99.8–100%, and, at a different iron loading, lowered the onset temperature from 530 to about 425 °C [40]. Steam can be incomplete: on Ni/CeZrO₂, about 12% of the carbon remained because nanotubes resisted gasification [35]. On Fe/CaO catalysts made from red mud and carbide slag, where CaO captures the CO₂, steam regeneration kept 89–93% of the first-cycle conversion over eight cycles [127,128], and sieving before gasification recovered part of the carbon as a sodium-ion anode material of 392 mAh g⁻¹ [129]. The gap between thermogravimetry and reactor widens with scale: in a kilowatt-scale solar reactor cycling Ni/Al₂O₃ between decomposition and CO₂ gasification, 99.8% of the carbon was removed in TGA but only 77.0% in the prototype [130]. Full oxidative regeneration can also weaken the particles: Ni/Al₂O₃ sintered on its first air regeneration and Ni/SiO₂ attrited, which led the authors to recommend partial regeneration [131].
Hydrogen offers a route that produces methane rather than COₓ. Short hydrogen pulses at 550 °C reactivated bulk nickel over 22 cycles using about 6.3% of the hydrogen produced, and doubled catalyst life in a membrane reactor at the cost of about 23% of it [43]. Small oxidant co-feeds act as continuous regeneration: 5% CO₂ in a Fe/Al₂O₃ fluidized bed doubled the net solid carbon from 2.43 to 4.98 g per g Fe in 1 h [39]. Non-thermal plasma removed only surface carbon, at most 38.6% [133].
Regeneration solves the catalyst problem by giving up the carbon. With oxidants its products are CO, syngas or CO₂ instead of a saleable solid; with hydrogen it consumes product and makes methane. At process scale, one design ships the carbon-loaded catalyst to a central plant, burns the carbon in oxygen with CO₂ storage and returns 95% of the catalyst; in that model the catalyst cost fell from 0.31 to 0.02 € per kg H₂ and the hydrogen cost from 3.39 to 3.07 € per kg, at the price of higher capital and electricity costs [134]. Activity above 100% after regeneration, reported in three studies, is a measured gain over the first cycle; it is attributed to restructuring only where the source shows it, and should be reported separately from retention (Section 8).

4.6. Comparison

What a step does to the carbon itself is rarely reported. Nineteen before-and-after Raman pairs from 10 studies are available (Figure 6c), and they do not move in one direction. Oxidation followed by sulfuric acid lowered ID/IG of nanotubes from 0.47 to 0.27–0.36 [104], and mild oxidation in 1% O₂ from 0.70 to 0.50 [92], because both remove disordered carbon preferentially. Annealing at 2800 °C lowered it from 0.73 to 0.29 [101], whereas annealing plasma carbon at 500–1500 °C raised it slightly, from 0.87–1.01 to 0.92–1.14 [88,105]. Nitric acid raised it on carbon onions, from 0.40 to 0.49 [100], but lowered it slightly on nickel-grown nanotubes, from 0.84 to 0.78 [45], and an anodic leach raised it from 0.73 to 0.84 [101]. Regeneration leaves a carbon whose order depends on the gas: oxygen at 850 °C lowered ID/IG on an iron catalyst from 0.87 to 0.64 [37], whereas CO₂ cycling raised it from 0.52–0.63 to 0.69–0.72 on two of four Ni/CeOₓ catalysts and left it within 0.03 on the other two [81]. Purification can therefore raise or lower the grade of the carbon, and the change has to be measured, not assumed; Supplementary Figure S3 shows how rarely recovery, purity, residual metal, Raman, carbon form and a use test are reported together for each route.
Table 2 sets the routes side by side on the quantities that decide whether carbon becomes a product and the catalyst can be reused: how much carbon is recovered, how clean it is, what happens to the catalyst, and what limits the route.
No route yet combines high carbon recovery, low metal and salt content, retention of the catalyst and a reported energy or reagent cost. Table 3 sets out the studies that come closest, as chains from catalyst to cost with each link marked as measured, modeled or missing. Of the eight condition rows that report both growth mode and metal in the carbon (Section 3.4; in one of them as catalyst mass in sieved carbon [98]), one also reports the carbon mass kept through washing [51], and none reports a carbon balance over the process; the most complete chains come from studies that measured removal directly.
The engineering question of how to withdraw carbon continuously is taken up next.

5. Continuous Carbon Withdrawal: Reactor Engineering

A plant making 100 t of hydrogen a day must remove about 300 t of solid carbon a day from a reactor at 600–1200 °C. The engineering dataset shows how far laboratory and pilot reactors are from doing this. Of the 71 experimental reactor rows, 35 describe batch operation with no carbon withdrawal, and only 6 report the fraction of the carbon produced that was actually recovered.

5.1. Why Fixed Beds Fail

Packed beds fill with carbon. A wood-charcoal bed held 44–70% conversion for up to about 35 h with a stable pressure drop, but the deposit formed a dense graphitized block of 0.68 m² g⁻¹ that plugged the reactor on cooling [135]. Modeling of a carbon-particle bed predicts that deposition concentrates at the inlet and can cut voidage from 0.38 to 0.11 within 20 min at 1 s residence time [136]. With 40 wt% Fe/Al₂O₃, a fixed bed reached a pressure drop of 40 kPa within 35 min and had to be stopped, while the same catalyst in a fluidized bed gave 10.68 g C per g catalyst with negligible pressure drop [52]. Catalyst coated on the wall avoids clogging if the catalyst loading stays below about 10 mg cm⁻³: a coated tubular reactor ran 46.4 h and made 62 g C per g catalyst, against 1.8 h and 0.3 g C per g catalyst in a fixed bed, but the carbon still carried nickel at its tips [137]. Without a catalyst, carbon deposits on hot walls and in exit lines: in an alumina tube most carbon formed graphitic sheets on the wall [138], and in a steel tube at 950 °C aromatic condensate blocked the exit line after 3 h [139].

5.2. Fluidized and Moving Beds

Fluidized beds tolerate carbon growth for longer, and several developers favor them (Section 9), but particles grow as carbon accumulates. With a commercial Ni/SiO₂ catalyst, carbon yields exceeded 70 g C per g catalyst at 550 °C in 70% CH₄ with 5% H₂, and in a run on pure methane the particles grew from 550 µm to over 1000 µm, raising the minimum fluidization velocity above 2 m s⁻¹; segregation and defluidization then drove deactivation, and very high space velocities, with only about 20% conversion, were needed to keep the bed moving [140]. Porous Fe/Al₂O₃ can circulate as a carbon carrier only while its carbon stays below about 10 wt%; above that, particles crack and the bed expands [141].
The longest catalytic fluidized-bed run in the dataset used carbon that left the bed on its own. In a 6 cm bed of 500 g Fe–Al₂O₃ at 700 °C on 10% methane, carbon-laden fines began to elutriate steadily after about 10 h and were caught on two outlet filters swapped every 4 h. The abstract reports conversion above 80% for 160 h during a 230 h test; the results section gives above 80% for 165 h and above 30% for 270 h, and its figure spans 280 h with cycles [142]. The fines carried catalyst with them and were collected, not separated and returned. Carbon-sphere supports that shed carbon by abrasion ran 72 h without activity loss, but a second run was 40–50% slower, which the authors attribute to losing 5–15% of the catalyst mass per cycle in separation and handling [97]. Two-stage beds at different temperatures extend life: Ni/Cu/Al₂O₃ ran about 17 h with conversion falling only from 43.6% to 36.5% [143]. Computational fluid dynamics–discrete element method (CFD–DEM) modeling shows that withdrawing particles continuously from the bottom of the bed, with a catalyst residence time of about 12 s, holds deactivation at a plateau and keeps the bed fluidized, while a batch bed turns into a packed bed [144]. Carbon has also been withdrawn continuously from a fluidized bed by letting carbon and catalyst overflow together, at up to about 5 kg of carbon a day, as nanotubes, on Ni–Mn/Al₂O₃ in runs of 5–7 h, with fresh catalyst added in batches; the catalyst was not separated from the product [145]. The longest moving-bed operation found uses carbon as its own catalyst. Two pilot moving beds of about 10 and 15 cm diameter, charged with sieved pyrolytic carbon and run at 1000–1080 °C and about 0.8 MPa on pure methane, operated for more than 500 h in total, in continuous runs of 24–72 h; a screw at the bottom discharged carbon at 400 g h⁻¹ to hold the bed inventory, and 30–35% of the carbon formed was entrained and caught in a cyclone and bag filter [32]. Conversion was 20–37%; in a 24 h run it held at 23–24% for 13 h and fell to about 20% after 16 h, and carbon deposition on the reactor wall remained a problem. Because the catalyst is carbon, withdrawal needs no catalyst separation, but the grade of the product was not qualified. Other designs accept the catalyst loss and plan for it. In a cyclic biogas fluidized bed, the carbon nanofiber product, carrying about 6 wt% catalyst, was withdrawn after each run and fresh catalyst added to keep the inventory constant [146]. An autothermal fluidized bed that burns part of the hydrogen uses iron oxide at about $200 per t as an expendable catalyst; it reached a carbon-to-iron ratio of 8 after 3.5 h and carbon with 96% degree of graphitization, and the 67% loss of density and 68% gain in diameter of aged particles was proposed for their selective entrainment [93]. A flare-gas design leaves a sacrificial iron catalyst on silica fume in the product, which is sold unseparated as a concrete additive [147]. None of the experimental studies reviewed here demonstrates continuous withdrawal of a solid metal catalyst with separation and return of the catalyst.

5.3. Molten-Metal and Molten-Salt Bubble Columns

In molten media the active surface is renewed as carbon floats away, so encapsulation does not deactivate the catalyst in the usual sense; the difficulties move elsewhere. Molten Ni–Bi ran 170 h without deactivation [116], and a tin column with a quartz packing was disassembled “after 15 days of operation” without clogging, giving carbon of 99.30 wt% C and 0.70 wt% Sn; whether the operation was continuous is not stated [148]. The difficulty moves to the top of the column. In the same tin reactor, the carbon accumulated in the head space because no withdrawal was installed [148], and a Cu-promoted Ni–Bi melt ran 25–42 h until carbon filled the reactor [38].
The Karlsruhe liquid-tin program shows both the progress and the difficulty. Scaling the column 3.75-fold in volume did not lower conversion, but tin weeping through the gas inlet could not be prevented and had to be managed with prechambers and pressure control [102,149]. Pneumatic discharge removed only about 30 vol% of the carbon before the reactor head filled and the gas outlet was blocked; passive flotation–gravity discharge through an enlarged pipe ran longer, with the first carbon reaching the separator after 5.7 h [102]. Argon-assisted pneumatic withdrawal kept the head space clear in a related process, but lowered methane conversion [150]. A cold-flow analog of a molten bubble column compared four withdrawal devices: an overflow weir removed all floating particles but carried large amounts of liquid, implying melt loss; a pneumatic weir removed 55%, a venturi ejector 54% and a cyclone 28% [103]. Figure 8 shows these four concepts, the cold-flow rig on which they were tested, and a liquid-tin bubble column used for reacting tests. A process design assumes high-temperature multicyclones that remove at least 99% of the carbon [151], a figure no experiment has yet reached. Electrochemistry offers a lower-temperature molten route: chlorination of methane by molten-chloride electrolysis at 550 °C held about 30% conversion for 100 h, and the carbon was recovered by washing the solidified salt [152].

5.4. Heat and Solids

Heat and solids interact in every flowing-solids design. Heat enters through the wall in the externally heated pilots [32,142], by burning part of the hydrogen in autothermal designs [93], or through the melt in bubble columns. Wall heating conflicts with scale: in the moving-bed pilots, a 2.45-fold longer gas residence time in the wider tube raised conversion by only 5–10%, which the authors attribute to heat transfer [32], and hot walls are where carbon deposits (Section 5.1). Growing particles increase the minimum fluidization velocity and cause segregation [140]; carbon-laden carriers begin to crack when the carbon content exceeds about 10 wt% [141], necessitating the capture of fines downstream, as seen in the cyclones and filters used in the pilots mentioned above. In fixed beds, the pressure drop can terminate the run within minutes to hours [52]. No study reports these quantities together with a carbon and metal balance, so the operating window of a flowing-solids reactor cannot yet be defined from published data.

5.5. Benchmark and Gaps

Figure 9 compares the longest reported operation on each platform, drawing on both datasets and four further cited studies outside them, and distinguishes how the carbon left the reactor and whether a duration is a single run, an elapsed campaign or a cumulative total. The longest record is more than 500 h of cumulative operation across two pilot moving beds, in continuous runs of 24–72 h with carbon discharged throughout [32]; the next is a 15-day tin-column campaign of about 360 h whose continuity is not stated and which had no carbon withdrawal [148]. A review reports 2,500 h for a supported nickel catalyst at 550 °C [153], describing the run both as continuous and as cycled with regeneration; the value traces to a two-page magazine article by the developer group [154], not to a peer-reviewed study, and is not included in Figure 9. The longest uninterrupted run with carbon withdrawal is therefore 72 h, and the longest single test with withdrawal is the 230–280 h fluidized-bed test of Siriwardane et al. [142]. The quantities a process designer needs are almost never reported together (Table 4).
Platforms that make nanotubes as the product answer a different question from those that only withdraw carbon. In a floating-catalyst reactor, nanotubes leave continuously as an aerogel wound on a roller, with the iron catalyst nucleated from the gas phase leaving in the product (64–76% carbon in the laboratory, 95% in a 30 g h⁻¹ single-pass pilot); recycling the unreacted process gas raised the measured laboratory output from 0.13 to 0.17 g h⁻¹ while cutting waste, a feed with 33 vol% CO₂ simulating biogas lowered it to 0.10 g h⁻¹, and the multi-pass pilot at 30 g h⁻¹ is a model built on the single-pass pilot data, not a measurement [159]. In a fluidized bed, steam and argon pulses dislodged nanotubes from Fe/θ-Al₂O₃ over ten cycles, collecting 572 mg with about 86% carbon closure while initial conversion fell [44], and ultrasonication with magnetic separation recovered nanotubes from Ni–Cu–Zn/Al₂O₃ after the run, with the catalyst regenerated in batches [56]. These routes report different things: collection with the catalyst in the product, in-reactor dislodging with gradual loss of activity, and separation after the run with catalyst return. None yet reports throughput, product quality, residual metal and catalyst fate on one basis.
Six technical problems stand between these demonstrations and continuous operation for thousands of hours with closed solids and metal balances, and the engineering dataset shows how rarely each is measured: of 71 experimental reactor rows, fouling or plugging is reported in 35 (18 studies), attrition or fines in 17 (12), particle growth or defluidization in 12 (9), metal or salt carried out with the carbon in 17 (10), catalyst or melt make-up in 14 (10), and the fraction of carbon recovered in 6 (3); no study reports recovered carbon, carry-over and make-up for the same run, although all three set the cost (Section 6). First, solids must leave a hot, hydrogen-rich vessel without gas bypass or air ingress; the one pilot that describes its discharge used gas-sealed tanks and an explosion-proof design [32]. Second, particles grow as carbon accumulates, which shifts fluidization, raises the elutriation of fines that carry metal, and ends fixed beds by plugging (Section 5.1 and Section 5.2). Third, no metal-catalyst process separates catalyst from carbon at temperature and returns it to the reactor; every separation reported so far is made after the run, in batches (Section 3.5 and Section 5.5). Fourth, the issue of heat supply remains unresolved: at approximately 1000 °C, no externally heated surface remains free of coke in a reducing atmosphere, and electromagnetic heating only penetrates a few centimeters, which conflicts with the large diameters required for fluidized beds [1]. Fifth, molten media lose melt with the carbon and by entrainment, and salt caps that clean the carbon add salt that must itself be washed out (Section 4.3); these losses have been measured only over hours to days. Sixth, run lengths of hours to days, and even cumulative totals of a few hundred hours made up of day-long runs, cannot reveal slow losses of catalyst or melt, which matter most for cost. Analysis is not the limit: a loss large enough to matter is well above the detection limits of bulk methods (Section 6.3, Equation (3)), provided the carbon is collected and sampled over the whole campaign. Long fixed-bed runs exist (210 h on Ni–Fe [155]), but they use milligrams of catalyst and diluted feed, and say little about withdrawal. A pilot campaign of several thousand hours with full solids and metal balances is the experiment the field most needs.

6. Carbon Grade, Value and Hydrogen Cost

6.1. What the Routes Make

The removal route and the catalyst together set the grade of carbon a process can sell. Raman ratios do not separate the catalyst families clearly. At 532 nm excitation, family medians of ID/IG for as-produced carbon are 0.72 (Fe), 0.88 (Ni) and 0.97 (molten metal), each from three to five studies, and the spread within each family is wider than the differences between them (Figure 3a). Supported catalysts make filaments, platelets and shells rather than large graphite flakes; submicron graphitic powders suit lubricants and conductive additives, while battery and nuclear graphite are usually specified with particles tens of microns across [1], together with application-specific limits on crystallinity, surface area, impurities and morphology, so particle size alone does not define suitability. Molten metals give sheet-like graphitic carbon, but with tens of percent of metal until it is washed (Section 4.3), and molten salts give more disordered carbon holding trapped salt [85].
The markets for these grades differ by orders of magnitude in size and price. Carbon black sells about 16 Mt a year, carbon nanotube output is about 20,000 t a year, with quoted prices from a few dollars to hundreds of dollars per gram that depend on grade, purity and volume (catalogue or small-lot prices are not average realized prices at industrial scale), and bulk outlets are far larger but cheap. As theoretical substitution capacity, not demonstrated demand, carbon fillers in cement could absorb up to 160 Mt a year if priced near cement at about $160 per t, asphalt binder sells above $400 per t with demand above 128 Mt a year, and metallurgical coke demand is about 600 Mt a year [7]. These are the volumes and prices of the materials replaced, not markets demonstrated for pyrolysis carbon. High-value grades cannot absorb the carbon from hydrogen made at scale; bulk outlets can, at a fraction of the price [7,27]. The carbon need not always be separated for use. The spent iron–char catalyst, which has a Fe/C mass ratio of about 0.22, gasified in CO₂ far faster than metallurgical coke (70.7% conversion compared to 6.5% at 900 °C) and has been proposed as a steelmaking feed, thereby turning the separation issue into a qualification issue [160]; a similar argument applies to once-through iron-ore catalysts. A combined carbon–catalyst product intended for direct use needs its own qualification, separate from that of a purified carbon grade. Three levels of evidence should be kept apart: characterization of the carbon, a test in an application against a reference product, and qualification by a customer. Only 25 of the 95 experimental studies (26%) reach the second (Figure 2) and none reports the third, so most claims about value rest on characterization. Supplementary Table S5 sorts the application tests cited below by material class, treatment, loading, comparator and evidence level; carbon black, mixed nanotube–nanofiber products, carbon-coated slag, graphite and carbon fibre are different materials, and results do not transfer between them.
Recent application tests widen the bulk outlets. Nanocarbon deposited from methane on steel slag at 900 °C raised the 28-day strength of mortar by 26% at a dosage of 0.15 wt% [161], and microwave-plasma carbon was about 98% carbon by elemental analysis with half the surface area of a commercial conductive black, a characterization rather than an application test [162]. Fibrillar pyrolysis carbon replacing 5% and 10% of cement raised mortar compressive strength by at least 20% and 16%, while disk-like carbon gave little benefit, and the 10% replacement cut cement emissions by about 10% [163]. Nanocarbon grown directly on steel slag raised mortar strength by 15–18% at 0.15 wt% of the cement, with no separation step [164], and a mixture of nanotubes and nanofibers from Ni–Cu–Al catalysts stiffened asphalt binder at 2 wt% and improved its ageing resistance at some cost in ductility, with unpurified and acid-purified material performing similarly in the tests reported, so purification may be unnecessary for this use [165]. A spent catalyst with its carbon served as a microwave absorber, an outlet where retained metal is useful [166], and methane-derived carbon infiltrated into carbon-black-loaded precursors gave structural carbon fibres at about $13.5 per kg [167]. For batteries, purified iron-ore carbon outperformed natural graphite as an anode (120.4 against 70.2 mAh g⁻¹ at 1C) and carbon black as a cathode additive [114]. Two cautions apply. A screening health-risk assessment found the handling of nano-carbon at a steel plant acceptable only with dust control, and estimated that the carbon of one large plant would fill a landfill site in about a month [168]. And graphite made from natural gas needs graphitization energy, whose source dominates its life-cycle advantage [169].

6.2. Hydrogen Cost with and Without Carbon Sale

Figure 10 places 25 selected published estimates from 21 studies on one currency basis, 2023 US dollars: each study’s base case or, where it gives none, the case named in Supplementary Table S4, which also states whether each value is a levelized cost or a minimum selling price, with its scale, gas and electricity prices, credits, carbon grade and fraction sold. Without carbon sale, the estimates span $1.7–8.2 per kg H₂ (20 results), with catalytic solid-bed routes at $1.7–6.6, molten metals at $2.1–3.7 and molten salts at $2.6–3.7. With carbon sold at the price each study assumed, they span $0.8–4.1 per kg (15 results). Most studies sell all carbon at $150–1,810 per t; exceptions are Lumbers et al. [170], who sell 10% of the carbon at $10,000 per t, Tamarona et al. [171], whose value is a model bound that sells 50% and disposes of the rest, Alhamed et al. [33], who use a demand-limited market model, and Yousef et al. [172], who sell 58.5% of the carbon (90% separated, 65% marketable). Ten results from seven studies report both values for the same case, but only five of them, from four studies, differ by the carbon credit alone with all carbon sold; for these the reduction is $0.7–2.3 per kg [173,174,175,176]. The three demand-limited pairs yield about $1.6 per kg [33], and one plasma study provides $7.1 per kg because its comparison also credits steam and pairs a range midpoint with its best case [177], and one partial-sale pair, with 58.5% of the carbon sold at $200 per t, differs by about $0.3 per kg [172]; Figure 10 marks these classes separately. Few cases reach the $1–2 per kg range that Le et al. [1] cite as the total cost of unabated SMR hydrogen; all but one of these cases involve carbon sales, while the exception is a small plant that uses inexpensive associated gas [176]. The comparison is contextual, since hydrogen specification, regional costs and boundaries are not aligned with those of the SMR estimate. Escalation does not align feedstock prices either, which differ widely between studies (Supplementary Table S4): at about 0.21 MMBtu of methane per kg of hydrogen, a difference of $3 per MMBtu alone moves the cost by more than $0.6 per kg.
Where a study reports both values and the carbon price, the cost falls by $0.30–0.38 per kg H₂ for each $100 per t of carbon price [173,174,175,176], and by $0.39 where a steam credit is included [177]. The lower end of that range is set by stoichiometry. Each kilogram of hydrogen formed comes with 2.98 kg of carbon, so the reduction in LCOH due to the carbon is
ΔLC = mC × (fₛ × P − fₜ × Cₚ)/1000 (USD per kg H₂)
where mC is the carbon formed per kilogram of hydrogen delivered (2.98 kg when all hydrogen formed is delivered, more when part is burned or lost in separation), fₛ the fraction of that carbon sold at price P (USD per t), and fₜ the fraction treated, at a purification and handling cost Cₚ per tonne treated. ΔLC is the LCOH reduction from carbon; it is positive when the revenue from sold carbon exceeds the treatment cost. The variables fₛ and fₜ are both fractions of the carbon formed and are set independently, because carbon may be sold untreated, or treated and not sold. Disposal costs and other co-product credits are separate terms. With mC = 2.98, fₛ = 1 and Cₚ = 0, the credit is $0.298 per kg of hydrogen formed per $100 per t; this figure is an illustrative revenue sensitivity for pure methane with all carbon sold and no treatment cost, not a measured credit, and it matches the lowest slopes. This floor holds for pure methane with all carbon sold: ethane and heavier hydrocarbons raise mC (about 3.1 kg C per kg H₂ for 10% ethane), and partial sale or recovery (fₛ < 1) lowers the slope below 0.298, as in a solar molten-salt design that sells 58.5% of its carbon and gains $0.17 per kg H₂ per $100 per t [172]. Slopes above 0.298 arise when part of the hydrogen is burned for process heat, so that mC exceeds 2.98, as in Cheon et al. [173], where hydrogen makes up 40% of the fuel burned for heat and methane the rest, when part of the hydrogen is lost in purification, as with 90% recovery in pressure-swing adsorption in Tiam et al. [176], or when other co-products are credited. The equation also shows what most studies leave out. The parameters fₛ, fₜ, and Cₚ are determined by market size, carbon recovery (Section 5), and the removal route (Section 4), respectively; however, almost every techno-economic analysis (TEA) assumes a sale price that includes full recovery without accounting for separate purification costs.
Break-even carbon prices follow. The cost of carbon needed to break even was 306 € per t, with hydrogen sold at 1.6 € per kg [186]; thermal decomposition matched reforming at a carbon value of 310 € per t, with a CO₂ allowance of 10 € per t [188]; molten Ni–Bi with a salt layer needed more than $200 per t of carbon without a CO₂ price [184]; methane pyrolysis at 20 t of hydrogen a day needed more than $500 per t of carbon black [178]; and carbon revenue of 500–750 € per t gave hydrogen at zero cost across several routes [189]. These prices sit above bulk outlets ($160–400 per t) and below the prices of specialty carbons, which is why the grade matters.
Applied to the substitution scenarios above with mC = 2.98 and full sale, Equation (1) provides credits of about $0.48 per kg H₂ for cement filler at $160 per t and, as an upper bound based on the bitumen price, $1.19 per kg for asphalt at $400 per t before purification. A route that needs acid washing or high-temperature treatment to reach a saleable grade must recover that cost from the margin between the grade’s price and these bulk values. Within the reviewed corpus, only one study models purification as a separate scenario. For nanotubes made from biogas, purification without catalyst recovery raised the minimum selling price of the solid product from $9 to $10.30–21.42 per kg and its footprint to up to 11.45 kg CO₂-eq per kg; recovering 90% of catalyst and acid at a yield of 10 g per g lowered the price to $3.95–6.26 per kg, a combination the authors note no continuous plant has shown [190]. These are modeled minimum-selling-price scenarios in which recovery and yield change as well, so their difference is not an isolated treatment cost; it indicates only the order of magnitude of Cₚ for a specialty grade, about $1,300–12,400 per t of product, and not for bulk carbon. Another TEA includes acid washing and metal recovery in its total process cost without reporting them per tonne [96]. A route-resolved comparison is therefore a calculation that the field has not yet been able to do with measured inputs.

6.3. Catalyst and Melt Make-Up

Losing catalyst or melt is the other large cost, and it is the one least measured. For a Ni–Bi bubble column, raising the metal lost with the carbon from 0.001% to 1% changed the hydrogen cost by about $0.4 per kg, whereas for a tellurium melt the same change was far larger [179]. Shortening the inventory life of a Ni–Bi melt from half a year to ten weeks raised the cost from $1.67 to $2.83 per kg in one case [174]. Raising the metal loss from 0.1% to 5% raised the carbon price needed for $1 per kg hydrogen from $1.49 to $6.76 per kg of carbon for a Ni–Pd catalyst, but only from $1.39 to $1.44 for Ni–Cu [96]. A stochastic analysis spanned $0.44 to $21.49 per kg between its optimistic and pessimistic scenarios, which differ in catalyst loss (0.001 to 0.62 kg per kg H₂) and also in gas price (0.6 to 18 USD per MMBtu), so the range is not an effect of catalyst loss alone [191]. A techno-economic model of a 100 t per day fluidized bed estimated that 89–229 kg of fresh nickel catalyst an hour would be needed to hold an average deactivation factor of 0.85 [171]. All of the sensitivities in this paragraph are model results, not measurements.
For catalyst used once through, with no recovery, Le et al. [1] give the make-up cost per kilogram of hydrogen directly:
Cmu = pcat × mC/RC/cat (USD per kg H₂)
where pcat is the catalyst price (USD per kg), mC = 2.98 kg of carbon per kg H₂, and RC/cat is the carbon-to-catalyst mass ratio of the spent solids. Figure 11 places the measured ratios from this dataset on that framework. The median of the study maxima, the highest ratio reported in each study, is 1.8 kg C per kg catalyst (95% bootstrap interval 0.4–9.2; interquartile range 0.4–9.3; 16 studies, all supported metal catalysts), above the ratio of about one that Le et al. take as typical of supported catalysts but within the same order; these are study maxima, the carbon formed by the end of runs of median 2 h (0.15–100 h for the study maxima; the shortest run in the dataset lasted 5 min), and only two of the 16 runs went to deactivation (four ended with conversion falling, one still active, and nine do not report it), so they understate what the catalysts could hold over their life and are not plant ratios; no unsupported metal, ore or carbon catalyst in the harvest-evidence dataset reports a yield on this basis. At $5 per kg of catalyst, the upper guardrail Le et al. suggest, this gives a once-through make-up cost of about $8.3 per kg H₂. This is an illustrative estimate from the reported laboratory yields, not a cost at a demonstrated continuous-plant ratio. If these catalysts would have kept accumulating carbon on the same basis, it overstates their make-up cost, but the short runs do not establish a bound for plant operation, where feed, conversion and deactivation differ. A rate alone cannot replace the ratio (averaged over these runs, 0.1–14 g C per g catalyst per hour), because make-up depends on the carbon formed over the whole life of the catalyst. The framework assumes that all carbon leaves on the spent catalyst, that the spent catalyst has no salvage value and that metal left in the carbon does not lower its price; the first two overstate the cost and the third understates it. The figure depends on the aggregation rule: excluding runs of 1 h or less gives about $7.4, and the median of each study’s median rather than of its maximum about $14 per kg. To keep the make-up cost below $1 per kg of H₂ at that price, a ratio above 15 is required; only one of the 16 studies achieves this in runs of 50–100 h [43]. Catalyst recovery lowers this cost only by the fraction of the inventory that is returned with its activity intact. In the one process model that costs recovery, returning 95% of an iron catalyst cut its cost from 0.31 to 0.02 € per kg H₂ [134]; experimental studies report neither the fraction recovered nor the activity it keeps over many cycles. For molten metals, the equivalent quantity is melt loss per tonne of carbon, which no experiment reports directly; the 0.70 wt% tin found in carbon from a tin column [148] would already be a measurable melt make-up if not recovered. The cost model of Von Wald et al. [180] reports the strongest sensitivity: in its Ni–Bi case, which delivers hydrogen at $1.75 per kg without carbon revenue, contamination of the carbon by 0.0001 wt% of melt raises the levelized cost of the delivered energy from $11.09 to $38.50 per MMBtu, and 0.0005 wt% to $148. A direct mass balance does not reproduce these results: at 2.98 kg of carbon per kg of hydrogen and a melt price near $10 per kg, 1 ppm of melt in the carbon costs about $0.00003 per kg H₂, and 1 wt% about $0.3 per kg, in line with the $0.4 per kg that Kim et al. [179] report for 1% loss. The reported sensitivity therefore depends on how that model defines its loss term; what transfers is the direction, that melt leaving with the carbon is a first-order cost. The carbon from the molten-tin pilot above contained about half its mass as tin [122].
Catalyst or melt that leaves with the carbon can be costed in the same way. If the carbon product holds a mass fraction w of metal or catalyst and a fraction r of it is recovered, the loss per kilogram of hydrogen is
mloss = mC × w/(1 − w) × (1 − r) (kg per kg H₂)
and its cost is mloss times the price of the metal or catalyst. Because of the factor w/(1 − w), the loss rises steeply with contamination. For the unwashed carbon of bismuth-based melts (w = 0.52–0.83 [59,83]) and no recovery, mloss is 3.3–14.5 kg of metal per kg H₂, so each dollar per kilogram of melt price adds $3.3–14.5 per kg H₂; under a salt cap (w = 0.022–0.05 [59,83]) it falls to 0.07–0.16 kg, or $0.7–1.6 per kg H₂ at an illustrative $10 per kg. Both are losses before any recovery, which is why molten-metal routes depend on salt caps, washing and metal return together. Equation (3) also sets what a mass balance must resolve: a loss worth $0.10 per kg H₂ at $5 per kg of catalyst is 0.02 kg per kg H₂, or about 0.7 wt% catalyst in the carbon, far above the detection limits of bulk ICP or XRF, so losses that matter are measurable once the carbon is collected and analyzed over long campaigns. No continuous operation in the reviewed evidence reports a measured catalyst or melt loss rate, so every sensitivity in this section is a model result. Melt loss also carries emissions: in one cradle-to-gate assessment, 1% Ni–Bi in the carbon added about 1.75 kg CO₂-eq per kg H₂ through replacement of the melt, against 0.002 kg at 0.001% [179] (Section 9.3).
Carbon value and catalyst or melt loss therefore pull against each other through the removal route. A route that recovers clean carbon without losing catalyst raises fₛ, lowers Cₚ and raises the carbon-to-catalyst ratio at once; a route that burns the carbon or carries metal out with it loses on all three. Machine learning is increasingly proposed to identify catalysts that do better on these quantities; the next section asks whether it can.

7. Machine Learning: What Is Validated, and What Is Missing

Machine learning has entered the field quickly: almost two-thirds of the 23 machine-learning papers audited here appeared in 2025 or later. The audit covered the 23 ML papers found by the machine-learning queries of Section 2.1 and by citation searching. Two of them [192,193] use the same data and are counted as one study, leaving 22 studies; 21 of them train a model: 15 on methane decomposition or pyrolysis (the remaining study is a perspective without a model), 4 on carbon nanotube synthesis from other carbon sources, and 2 on related catalytic systems used as methodological benchmarks. For each study the audit recorded, with a quotation from the paper, the data source, sample size, how the data were split (random by row, ungrouped k-fold, grouped by source or chemistry, time or extrapolation, or not stated), whether the model was tested on data or experiments not used in training, the reported accuracy, the targets and whether data and code were shared (Supplementary Table S1, which identifies each paper, model and dataset family; [106,192,193,194,195,196,197,198,199,200,201,202,203,204,205,206,207,208,209,210,211,212,213]).

7.1. Validation Practice

Thirteen of the 21 studies split their data randomly by row or by ungrouped k-fold cross-validation, and for nine of them this is the only test; six do not state how the test set was drawn. Only one model trained on literature-compiled methane-decomposition data also groups the data before splitting: on 372 carbon-yield observations, grouping identical catalyst formulations lowered R² from 0.987 under random five-fold cross-validation to 0.878 ± 0.117, and the authors warn that random-split scores should not be read as generalization [212]. Another trained a neural-network surrogate on 3,840 runs of the authors’ own fluidized-bed model, with a random split and no experimental data [211]. This matters because these datasets contain many rows from each run. The largest compilation digitized conversion against time on stream from 26 papers into 2,736 rows and used shuffled cross-validation with time as an input [200]; another reused the data with a random split and imputed missing target values [203]; a third added 372 synthetic zero-time rows to 372 measured carbon yield rows [197]. Without grouping, points from one run can sit on both sides of the split. The papers do not provide split indices, so this is a risk of leakage that cannot be checked from outside; if it occurs, R² values of 0.997–0.9999 measure interpolation along a curve rather than prediction for a new catalyst. In two of these studies the hyperparameters were also tuned on the full dataset. One study trained on its own thermogravimetric runs kept two temperatures out of training: networks that fitted the training runs closely oscillated when forecasting the unseen runs, and only some generalized [213].
Small datasets show the same pattern. Three studies report test R² above 0.95 from 46–68 data points with no grouping and no external test [192,201,208]. The two papers by Almansour et al. [192,193], using the same 66 points from five sources, report R² of 0.9992 and 0.927 for the same target. A methodological benchmark found that feature rankings become statistically undetermined near 100 data points [206], which places the feature-importance claims in these small studies in doubt.
Apart from that run-wise hold-out, grouped splits appear only in density-functional-theory (DFT) studies, and they show what is at stake. On a database of 10,950 single-atom-alloy surfaces, random five-fold cross-validation gave R² 0.993 with every host, dopant and facet present in both training and test sets; leaving one dopant out cut R² to about 0.67–0.74 [194]. Tests outside the training data are of three kinds that differ in strength: computational tests on held-out groups of DFT data, as above; a single new experiment after training on literature data, which only two literature-trained methane-decomposition models report [197,200]; and prospective experimental validation throughout, which only closed-loop autonomous experiments on nanotube growth from ethylene achieve [209,210]. The 10,950-entry single-atom-alloy database used by Faisal et al. [194] was itself generated by an earlier machine-learning screen trained on 623 DFT values [106]. Three of the 21 studies share both data and code.

7.2. Targets

The models predict methane conversion, hydrogen yield, carbon yield, nanotube diameter and C–H activation barriers; one forecasts the carbon accumulated on an Fe/C catalyst over time [213], the quantity behind the carbon-to-catalyst ratio of Section 6.3. No model in the audited studies predicts carbon detachability, residual metal in the carbon, regeneration, catalyst lifetime or deactivation, or cost. Carbon structure appears as a target in only a few studies: Raman ratios with no reported accuracy [198] or with 22% mean absolute percentage error for non-methane nanotube films [207], and XRD crystallite size from 12 data points [195]. Within the audited set, the quantities that Section 3, Section 4, Section 5 and Section 6 identify as decisive are absent from the ML literature, largely because they are absent from the experimental literature it learns from.
A descriptor-driven, closed-loop search for Co-based quaternary molten alloys, which combines data mining with computation and experiment, was retrieved by the search but not classed as a model-training study; it too targets activity rather than carbon or melt properties [214].

7.3. What Would Make ML Useful Here

Four changes would make models in this field credible and relevant. Splits should be grouped by source paper and catalyst, with time-series points kept together, and a model should be judged on held-out catalysts, not held-out rows. Hyperparameters should be tuned without touching the test set. At least a small external test, on new experiments or on papers published after the training data, should be standard, and data and code should be released. And the targets should move toward harvest: carbon-to-catalyst ratio of the spent solids, metal content of the carbon after removal, carbon recovered, activity after regeneration, and run length. Until then, the published models cannot guide catalyst or process design for harvest. Datasets like the one in this review, which includes the reporting checklist in Section 8, are necessary for such models. Closed-loop experimentation, already shown for nanotube growth, is the most direct route to data of this kind.
How the data are structured matters as much as how much there is, and assembling the datasets of this review suggests five rules. First, records should be hierarchical, from study to catalyst sample to run to time point to each removal or regeneration step, so that splits can be grouped and time series kept intact. Second, every value should carry its basis, unit and method: carbon per gram of fresh catalyst or of metal, metal by bulk ICP or by local EDS, activity measured at a stated time in a stated cycle. Third, runs stopped before deactivation should be flagged as censored rather than treated as lifetimes; of the 16 studies behind Figure 11, two ran to deactivation and nine do not report the end state, so a lifetime target calls for survival-type models, not regression on the last value. Fourth, each value should keep a locator to the page, table or figure it came from, as Dataset S4 does here, and failed or negative runs should stay in. Fifth, records should follow community metadata models rather than new ones: CoreMeta4Cat defines the minimum information on catalyst, reactor and conditions in machine-readable form [215], and CatTestHub combines benchmark activity data with characterization and reactor configuration under FAIR principles [216]. Consistency can matter more than size: a small oxidative-coupling dataset measured on one set of equipment supported useful composition–performance models [217]. The targets to record are those of Section 8: the carbon-to-catalyst ratio with its end state, the metal in the carbon after removal, carbon recovered, activity after each regeneration cycle and metal lost per cycle.

8. A proposed Reporting Checklist

The comparisons in Section 3, Section 4, Section 5 and Section 6 were limited less by the number of studies than by what they report. Parts of a standard exist: productivity metrics for catalysts [15], kinetic reporting [28], ASTM International (ASTM) tests for carbon black grades [27], and a proposed standard set of analyses for carbon from natural-gas pyrolysis, covering density, particle size, oil absorption, surface area, thermogravimetric and temperature-programmed oxidation for carbon content and residual catalyst, XRD, Raman and electron microscopy [218]. These cover the carbon or the kinetics; kinetic guidelines also ask for the metal content of the carbon co-product [28]. Reviews call for standardized certification of the carbon and for quantified catalyst and melt losses [8,26], but none sets out what to report on removal, regeneration or catalyst consumption. Table 5 proposes a reporting checklist in four tiers that builds on them; Tier 1 adopts the carbon characterization of Riley et al. [218] where it applies. Each tier applies when a study includes that step, so a catalyst-screening paper needs only the first.
Three items would do most to make future studies comparable. The first is the carbon-to-catalyst mass ratio of the spent solids, at deactivation or with the time on stream and the conversion at the end, together with the metal content of the carbon after the chosen removal step; these two numbers place any catalyst on the make-up cost framework of Figure 11 and on the design-for-harvest map of Figure 5. The second is a carbon mass balance across removal, so that recovery is reported rather than inferred. The third, for techno-economic studies, is LCOH reported both with and without carbon sale, with the purification cost stated separately; this alone would allow the route-resolved comparison that Section 6 could make only with assumed inputs.
Applied to the present dataset, the standard shows how far practice has to move. Only 8 of 95 experimental studies report carbon yield, residual metal, and Raman together, and 3 of these also report surface area. Journals could ask for Tiers 1–2 as Supplementary Material at little cost to authors, since most of the measurements need only routine TGA, ICP, Raman and mass balances. A combined carbon–catalyst product intended for direct use should be reported as such, not as a carbon grade.
If only a core set can be required, six items make two experimental studies comparable: (i) carbon per gram of fresh catalyst with its basis, the time on stream, the conversion at start and end, and whether the run reached deactivation; (ii) feed composition and dilution, temperature, pressure and space velocity; (iii) the metal content of the carbon after the chosen removal step, by a bulk method with its detection limit; (iv) the carbon recovered across that step, from a mass balance; (v) for regeneration, first- and last-cycle activity measured at a stated time, and metal lost per cycle; and (vi) the carbon form, from microscopy together with XRD or Raman with laser wavelength and fitting. Items (i) and (iii) alone place a catalyst on Figure 5 and Figure 11 and, through Equations (2) and (3), on cost. Tier 5 extends the checklist to studies that report emissions (Section 9.3), and every tier is most useful when released in the machine-readable form described in Section 7.3.

9. Industry Status and Outlook

9.1. Where the Developers Stand

Companies developing methane pyrolysis rarely publish catalyst consumption, conversion, or carbon-removal data, so the status below rests on company releases, filings, and trade press, and should be read as company claims (Table 6; Figure 12). Peer-reviewed work by developer teams is cited where it exists.
Two moves stand out. Several developers favor moving-particle designs, fluidized and moving beds, in Hazer’s case, with a cheap once-through iron-ore catalyst. The molten-media developer Graphitic Energy has entered a scale-up collaboration with an engineering firm. The dataset is consistent with both moves: fluidized and moving beds are the only platforms that can carry growing solids out of the reactor (Section 5.2), and a cheap catalyst that leaves with the carbon avoids the need to separate them, provided the carbon can be sold with the catalyst in it or the catalyst costs well under the $5 per kg guardrail in Figure 11.

9.2. What Industry Names as the Problems

The engineering problems that developers report are not catalyst activity. They are moving carbon-laden solids for thousands of hours, supplying heat at 900–1200 °C without fouling, separating catalyst from carbon, and qualifying a new carbon product with customers. A trade review names avoiding fouling by carbon deposition and effective solids handling as the reactor requirements [225], and Hazer states that qualification for commercial offtake takes years; for the quarter to September 2026 it reported no receipts from customers, purification of its graphite to above 99.99% for battery assessment, and tests with Boral showing that the graphite can replace part of the bitumen in heavy-duty asphalt [223]. Academic work mostly addresses other questions: clean fixed beds over hours, laboratory acid leaching after the run, and techno-economic studies with a constant carbon price. Each section of this review identifies data that academia could supply and industry does not publish: population-balance and CFD–DEM models of growing particles (Section 5), carbon mass balances across removal and purification costs (Section 4 and Section 8), and catalyst make-up by carbon grade (Section 6).

9.3. Emissions Accounting

The pyrolysis reaction forms no CO₂, but the climate case for pyrolysis hydrogen rests on terms outside the reactor: how the reactor is heated, the methane emitted along the gas supply, the residues and make-up of carbon treatment and catalyst replacement, and what finally happens to the carbon. Equation (4) collects them per kilogram of hydrogen:
CIH₂ = Eheat + Eel + Esup + Emu + Etr − SC + 3.664 × fox × mC (kg CO₂-eq per kg H₂)
where Eheat and Eel are the emissions from fuel and electricity, Esup those of the natural-gas supply including leakage, Emu and Etr the embodied emissions of catalyst or melt make-up and of carbon treatment (acid, salt, energy), SC an avoided-product credit for the carbon under system expansion, and fox the fraction of the carbon later oxidized; 3.664 is the mass ratio of CO₂ to carbon. Under allocation, the first five terms are multiplied by the share of the burden assigned to hydrogen and SC is zero. Two terms set the scale. If all the carbon is eventually oxidized (fox = 1), the last term alone is 3.664 × 2.98 = 10.9 kg of CO₂ per kg H₂, comparable to the 9.3–11.5 kg CO₂-eq per kg H₂ reported for unabated steam reforming in most of the same studies (Figure 13); the climate benefit therefore depends on the carbon staying solid, not on the reactor. Methane leakage is the second: the reaction alone consumes 3.98 kg of methane per kg H₂, so each 1% of that methane lost upstream adds at least 0.01 × 3.98 × 29.8 ≈ 1.2 kg CO₂-eq per kg H₂ with the 100-year global warming potential of fossil methane, and about 3.3 kg with the 20-year value of 82.5 [233], before any methane burned for heat. This is why superiority over reforming with carbon capture requires upstream leakage below about 0.5% and very low-carbon electricity [8], and why a design that burns the carbon with CO₂ storage can still reach direct emissions of less than 1 kg of CO₂ per kg of H₂ [134]. The comparison also depends on how the capture step is represented, because CO₂ separation by absorption or by adsorption on carbon sorbents carries its own energy demand and capture rate [234,235].
Published results are not comparable as they stand (Figure 13; Table S6). Of the 48 cost and life-cycle studies in the engineering dataset, 30 report greenhouse-gas emissions, and 26 of these are primary assessments. Five use a functional unit other than hydrogen (a kilogram of nanotubes, carbon fiber, syngas or methanol, or a megawatt-hour of electricity). Eight count only direct emissions, with or without purchased energy, 17 assess cradle-to-gate, and one does not state its boundary [175]; four state or vary a methane leakage rate, and eight state the global-warming-potential basis. The carbon is handled in three incompatible ways: most studies assign the whole burden to hydrogen; two allocate part of it to the carbon, one by mass, which leaves 18.8% of the burden on hydrogen [236], and one by economic value [169]; and two credit the carbon by system expansion [190,237]. The choice alone can more than halve the result: a harmonized assessment found 12.6 kg CO₂-eq per kg H₂ without credit at full conversion, equal to reforming, and about 5.1 kg with an avoided-product credit for carbon black, an advantage lost below about 50–55% conversion [237]. Heat supply matters as much: in one molten-media assessment, direct emissions ranged from zero with renewable electric heating and gas recycle to 19.8–24.6 kg CO₂ per kg H₂ when the purge gas was burned [174], and gasifying the carbon on site raised another study’s intensity from 1.3 to 6.8 kg [188]. Ten studies state what happens to the carbon (landfill in three [134,183,238], a named durable product in four [93,167,169,190], gasification in one case [188], sale or sequestration as a cost item only in one [171], and later oxidation, which the study notes would add emissions, in one [176]), and none assigns an oxidized fraction. Melt loss carries emissions as well as cost: 1% Ni–Bi in the carbon added about 1.75 kg CO₂-eq per kg H₂ [179].
Standards do not yet close these choices. ISO 19870-1, published in April 2026, sets the method for hydrogen emissions up to the production gate and admits both attributional and consequential approaches, the latter avoiding allocation by system expansion through substitution [241]; because its boundary ends at the gate, the later fate of a solid co-product falls outside it. The United States 45VH2-GREET model used for the clean-hydrogen production tax credit lists no methane-pyrolysis pathway and no rule for a solid-carbon co-product in its December 2025 version [242].
Policy adds a further condition. Under the European Union (EU) methodology for low-carbon fuels, fossil CO₂ emitted at the end of life of co-products must be counted. Solid carbon is considered not emitted only if it is permanently chemically bound in a product listed in Delegated Regulation (EU) 2024/2620, or stored under the requirements of the Union framework for permanent carbon removals [243]. The products listed so far in Regulation 2024/2620 are mineral carbonates in construction products [244], and the first permanent-removal methodologies, adopted in February 2026, cover direct air capture and bioenergy with carbon storage and biochar [245]; none covers solid carbon from methane pyrolysis. Whether fossil solid carbon in other products, such as asphalt, rubber, or electrodes, counts as emitted at end of life therefore depends on provisions that do not yet exist. Carbon end-use is a regulatory as well as an economic question.
Table 7 sets out minimum accounting rules that would make results comparable across studies and with competing routes; they extend Tier 5 of the reporting checklist (Table 5), and each answers a difference found in the assessments above.

9.4. Safety and Scale-Up

Scale-up adds hazards that laboratory studies rarely address. Hot methane and hydrogen at 600–1200 °C need tight seals and inerting at every solids transfer point; the 15 cm moving-bed pilot above was built explosion-proof, operated from a separate control room and discharged its carbon into gas-sealed tanks [32]. Fine carbon is a combustible dust that must be contained from discharge to storage, and catalyst fines carry nickel or cobalt into the product and the workplace. Molten metals and salts add corrosion, weeping through gas inlets [149] and spills, and acid purification leaves spent acid and dissolved metal to be treated or recovered (Section 4.2). None of the primary studies reviewed report measurements of dust, fugitive emissions, or waste streams. A readiness claim for any route should therefore state the scale, the run duration and whether these integrated operations were demonstrated; the evidence reviewed here supports a comparison of reported demonstrations and their gaps, not a readiness ranking.

9.5. The Gulf Region

The Gulf combines cheap natural gas, strong solar resources and large construction and steel sectors that could absorb bulk carbon. A techno-economic study for Saudi conditions estimated $0.9–1.18 per kg of hydrogen from a Ni–Bi molten-metal bubble column with solar-photovoltaic or mixed-grid electricity (24–33 USD per MWh), without carbon revenue, at a natural-gas price of $60 per t [185]; this regional case is not plotted in Figure 10, which shows the study’s base case (molten KCl–MnCl₂ salt, $2.59 per kg at European prices). It rests on the regional electricity and gas prices and financing assumptions of that study. A comparison of pyrolysis routes at 3,288 t H₂ per day with unified boundaries found median costs of $2.46, $2.67 and $3.78 per kg (2024 USD) for fluidized-bed, molten-salt and molten-metal reactors without carbon revenue, and $0.79–2.08 per kg with demand-limited graphite sales [33]. For comparison, SMR in Saudi Arabia is estimated at $0.44 per kg without and $1.54 per kg with carbon capture, as reported, at a subsidized gas price of about 1.3 USD per MMBtu [246]; these are regional scenarios, and their boundaries differ from those of the pyrolysis studies. No Saudi methane-pyrolysis project was identified in the company releases, filings, and English-language trade press searched (October–November 2026); the only regional deployment identified is the graphene unit at an ADNOC plant. For the region, the questions are where the carbon would go, whether bulk outlets in cement, asphalt and steel can be qualified at scale, and whether iron-rich industrial residues could serve as once-through catalysts.

9.6. Outlook

The evidence indicates a near-term path that relies on fluidized or moving beds, inexpensive once-through or durable regenerable catalysts, and carbon that is initially sold into the highest-value grade achievable by the route, with a transition to bulk outlets as volumes increase; this staged deployment was also proposed by Le et al. [1]. The same group has since shown an autothermal fluidized bed that burns part of the hydrogen for heat and, on iron ore, makes graphite with 96% graphitization in 2–5 µm flakes; runs lasted 3–3.5 h, and carbon removal by selective entrainment was proposed rather than shown [93]. Molten media remain attractive for separation but must show melt losses low enough not to dominate cost (Section 6.3). In every route, the step from pilot to plant depends on data that are not yet public: continuous operation for thousands of hours with full solids and metal balances.
The authors’ group at King Khalid University is working along these lines. Earlier work developed supported catalysts for methane decomposition: hydrotalcite-derived Ni–Fe–Cu catalysts optimized by design of experiments [79], Co/TiO₂–Al₂O₃ with a kinetic model [64], Cu–Zn-promoted Ni–Co–Al [63] and Co–Rh on mesoporous TiO₂ [62], building on catalysts for dry reforming and partial oxidation of methane (Section 3.1). Related work used date-seed biochar as a support for Ni, Ag, Ti and W catalysts [247], generated Ni–Fe and Ni–Ru nanoparticles in situ to form metal–carbon composites while producing hydrogen from biomass [248], developed composite supercapacitor electrodes [249] and reviewed MXene–polymer composites for supercapacitors and batteries [250]. Two projects now under way address the gaps identified here. The first develops Fe–Ni catalysts on nitrogen-doped biochar to control the morphology of the nanotubes formed with hydrogen, and to qualify these nanotubes as supercapacitor electrodes; it targets the carbon-to-catalyst ratio, residual metal after removal and electrochemical performance, reported together as in Table 5, and engineering routes for scaling up their production. The second develops a moving-bed reactor for continuous catalytic pyrolysis of methane, biogas and plastics, building on the group’s work on biomass–plastic co-pyrolysis [251] and on biogas production by anaerobic digestion [252], with carbon withdrawn during operation and the solids and metal balances that Section 5.5 identifies as missing.

10. Conclusions and Research Priorities

Methane pyrolysis makes three times more carbon than hydrogen by mass, and its viability depends on removing that carbon, keeping the catalyst, selling the product, and keeping the carbon solid. Read through that lens, the literature shows that the steps between catalyst and cost are usually not measured together. Of the 95 experimental studies that provide harvest evidence, 31 report on carbon purity, 36 report on residual metal, and 25 report on an application test; however, only 8 studies report on carbon yield, residual metal, and Raman together. The reported carbon form tracks the catalyst and its conditions rather than a fixed rule, and base growth under strong metal–support interaction is a design hypothesis for mechanical harvest, not yet a demonstrated route. Among removal routes, acid leaching gives the cleanest carbon at laboratory scale, salt caps cut the metal in carbon from molten media by an order of magnitude, and gasification restores activity only by consuming the product.
On the reactor side, the longest reported cumulative operation exceeds 500 h across two carbon-catalyst moving-bed pilots, in continuous runs of 24–72 h; no metal-catalyst process in the reviewed evidence has shown continuous withdrawal with catalyst separation and return, and carbon collected from a molten-tin pilot contained only about 48 wt% carbon. Fouling, fines, particle growth, metal carry-over, and make-up are each reported in at most half of the experimental reactor rows, and the fraction of carbon recovered is reported in only three studies. Selling the carbon lowers the hydrogen cost by about $0.30 per kg for each $100 per t, as stoichiometry requires, while catalyst or melt loss can add several dollars per kg: at the median of the laboratory study maxima of the carbon-to-catalyst ratio, 1.8 (16 studies, from runs of median 2 h, most stopped before deactivation), once-through catalyst make-up alone would cost about $8.3 per kg of hydrogen at $5 per kg of catalyst ($7.4–14 depending on the aggregation rule), a screening value rather than a plant cost, and unwashed carbon from bismuth-based melts would carry 3.3–14.5 kg of metal out per kg of hydrogen unless it is recovered. Only one study in the corpus models the purification of the carbon as a separate scenario, for a nanotube grade.
The environmental case rests on the fate of carbon. If all of it is later oxidized, it releases 10.9 kg of CO₂ per kg of hydrogen, comparable to unabated reforming, and each 1% of upstream methane leakage adds at least 1.2 kg CO₂-eq. Of the 26 primary assessments that report emissions, the 19 that give an absolute value per kilogram of hydrogen span 0 to about 25 kg CO₂-eq per kg H₂, mainly because the assessments differ in boundary, leakage, heat supply, and treatment of the carbon; none quantifies the fraction later oxidized, and neither the EU methodology for low-carbon fuels nor the US 45VH2-GREET model yet covers solid carbon from methane pyrolysis. None of the 21 machine-learning models audited, 15 of them on methane decomposition, targets carbon detachability, residual metal, carbon recovery, regeneration, catalyst lifetime, or cost; one forecasts carbon accumulation over time. These figures describe the published literature and its gaps; a quantified relationship between removal route, carbon fate, and value remains to be measured.
Six priorities follow.
  • Catalysts designed for harvest. Test whether strong anchoring with filament growth allows mechanical harvest, reporting the carbon-to-catalyst ratio at deactivation (or with the time on stream and the conversion at the end) and the metal content of the carbon after removal. A ratio above about 15 is needed for catalyst make-up below $1 per kg H₂ at $5 per kg of catalyst.
  • Removal with a mass balance. Report carbon recovered, catalyst recovered, residual metal and salt, and energy and reagent use per tonne of carbon, for every removal route.
  • Long runs with flowing solids. Pilot campaigns of thousands of hours on fluidized or moving beds and molten columns, with gas-sealed solids withdrawal, measured particle growth and fines, catalyst separation and return at temperature, and solids, metal and melt balances closed over the whole campaign, so that loss rates are measured rather than modeled.
  • Cost studies resolved by route and grade. LCOH with and without carbon sale, the fraction sold, the purification cost and the catalyst or melt loss per kilogram of hydrogen stated separately, so that Equations (1)–(3) can be evaluated with measured inputs.
  • Emissions accounted for the fate of carbon. Cradle-to-gate assessments per kilogram of hydrogen that report the leakage rate under both warming horizons, the heat source and the carbon treated three ways, and that state the end use and oxidized fraction of the carbon (Table 7); and qualification routes that allow durable carbon products to count as storage.
  • Machine learning on harvest targets, on data built for it. Hierarchical, machine-readable records with basis, method, censoring flags and source locators, following community metadata models; grouped splits by paper and catalyst, external tests, and released data and code; and targets that include carbon recovered, residual metal, regeneration and lifetime.
The datasets compiled for this review, released with it, are a starting point for all six; their sources not cited above are [253,254,255,256,257,258,259,260,261,262,263,264,265,266,267,268,269,270,271,272,273,274,275,276,277,278,279,280,281,282,283,284,285,286,287,288,289,290,291,292,293,294,295,296,297,298,299,300].

Supplementary Materials

The following supporting information can be downloaded at the website of this paper posted on Preprints.org. Figure S1: Search and selection flow; Figure S2: Reporting matrix by study; Figure S3: Evidence reported by removal route; Table S1: Machine-learning studies audited; Table S2: Sources of the two datasets with references; Table S3: Disposition of flagged rows; Table S4: Cost cases plotted in Figure 10; Table S5: Application evidence by material class; Table S6: Greenhouse-gas assessments coded by functional unit, boundary, methane supply, heat supply, carbon treatment and carbon fate; Document S1: Extraction schemas and quality-control reports; Document S2: Search strategy (PRISMA-S); Dataset S1: Master data extract, carbon dataset (102 sources) and engineering and cost dataset (101 sources), with the machine-learning audit and the coding of the emissions assessments; Dataset S2: Normalization of hydrogen costs to 2023 USD (CPI base, CEPCI sensitivity); Dataset S3: Extraction records (JSON), plotting and cost-normalization scripts, with readme; Dataset S4: Point-to-source manifest for every plotted value; Dataset S5: Search-audit workbook (search log, deduplication and screening ledger).

Author Contributions

Conceptualization, M.S. and M.K.A.M.; methodology, M.S., M.K.A.M., and M.D.; software, K.A.B.A. and M.D.; validation, N.M.M.A. and K.A.B.A.; formal analysis, H.A.A.O.; investigation, M.D. and N.M.M.A.; resources, M.D.; data curation, H.A.A.O. and K.A.B.A.; visualization, M.S. and M.K.A.M.; writing—original draft preparation, M.S.; writing—review and editing, M.S., M.K.A.M. and M.D.; funding acquisition, M.K.A.M. All authors have read and agreed to the published version of the manuscript.

Funding

This research was funded by the Deanship of Research and Graduate Studies, King Khalid University, through the Large Research Project under grant number RGP2/467/46.

Institutional Review Board Statement

Not applicable.

Data Availability Statement

The master data extract compiled for this review (Dataset S1), the cost-normalization workbook (Dataset S2), the extraction records with the plotting and cost-normalization scripts and a readme (Dataset S3), the point-to-source manifest for every plotted value (Dataset S4), the search-audit workbook with every screening decision (Dataset S5; bibliographic fields only, abstracts withheld under the database terms of use), the extraction schemas and the quality-control reports are provided in the Supplementary Materials; every plotted value can be traced to its source through these files.

Acknowledgments

The authors extend their appreciation to the Deanship of Research and Graduate Studies at King Khalid University for funding this work through the Large Research Project under grant number RGP2/467/46.

Declaration of generative AI and AI-assisted technologies in the writing process

During the preparation of this work, the authors used Grammarly and QuillBot for language editing, and SciSpace to search the literature, pre-screen database records, and extract values from the source publications into the fixed schemas. No generative-AI tool was used to create or alter images: the data figures were drawn with the scripts in Dataset S3, and the panels reproduced in Figure 4 and Figure 8 were cropped and scaled only. The authors defined the scope, schemas, and inclusion rules, checked the extracted values against the source publications as described in Section 2.3, revised the text, and take full responsibility for the content of the published article.

Conflicts of Interest

The authors declare no conflicts of interest.:.

Abbreviations

The following abbreviations are used in this manuscript:
Abbreviation Meaning
ADNOC Abu Dhabi National Oil Company
AI artificial intelligence
ASTM ASTM International
ASX Australian Securities Exchange
BET Brunauer–Emmett–Teller
CB carbon black
CCS CO₂ capture and storage
CEPCI Chemical Engineering Plant Cost Index
CFD–DEM computational fluid dynamics–discrete element method
CPI-U consumer price index for all urban consumers
DCFC direct carbon fuel cell
DFT density functional theory
DOI digital object identifier
EDS energy-dispersive X-ray spectroscopy
EU European Union
FAIR findable, accessible, interoperable and reusable
FB fluidized bed
FBR fluidized-bed reactor
GREET Greenhouse gases, Regulated Emissions, and Energy use in Technologies model
GWP global warming potential (GWP20 and GWP100: 20- and 100-year horizons)
ICP inductively coupled plasma
ISO International Organization for Standardization
JSON JavaScript Object Notation
LCOH levelized cost of hydrogen
MB moving bed
ML machine learning
MMR molten-metal reactor
MSR molten-salt reactor
NMR nuclear magnetic resonance
PRISMA Preferred Reporting Items for Systematic reviews and Meta-Analyses
PRISMA-S PRISMA extension for reporting literature searches
PSRI Particulate Solid Research Inc.
SMR steam methane reforming
SwRI Southwest Research Institute
TEA techno-economic analysis
TEM transmission electron microscopy
TGA thermogravimetric analysis
USD United States dollar
XRD X-ray diffraction
XRF X-ray fluorescence

References

  1. Le, S.; Moise, H.; Cargnello, M. A Perspective on Supported Catalysts for Methane Pyrolysis: Toward Hydrogen Production and Synthesis of Crystalline Carbon Materials. ACS Catal. 2026, 16, 9605–9617. [Google Scholar] [CrossRef]
  2. IEA. Global Hydrogen Review 2026; International Energy Agency: Paris; Available online: https://www.iea.org/reports/global-hydrogen-review-2026 (accessed on 11 November 2026).
  3. Shah, M.; Meena, S.; Mondal, P.; Kumar, A. Thermodynamic equilibrium modeling of gasification for syngas production from carbonaceous feed containing the sulfur impurity. Int. J. Chem. React. Eng. 2025, 23, 791–801. [Google Scholar] [CrossRef]
  4. Shah, M.; Kumar, A.; Chaturvedi, A.; Diab, M.A. Pioneering the green hydrogen revolution: Science, innovations, and industrial insights in algal biohydrogen production. Int. J. Hydrogen Energy 2026, 254, 156203. [Google Scholar] [CrossRef]
  5. Shah, M.; Mondal, P.; Nayak, A.K.; Bordoloi, A. Hydrogen from Natural Gas. In Sustainable Utilization of Natural Resources; Mondal, P., Dalai, A.K., Eds.; CRC Press: Boca Raton, FL, USA, 2017; pp. 81–120. [Google Scholar] [CrossRef]
  6. Chase, M.W., Jr. NIST-JANAF Thermochemical Tables. In Journal of Physical and Chemical Reference Data Monograph 9, 4th ed.; American Chemical Society and American Institute of Physics: Woodbury, NY, USA, 1998. [Google Scholar]
  7. Iorio, V.S.; Pedrazzoli, M.; Sala, G.; Lainati, A.; Lucini, F. Turquoise Hydrogen for a Circular Future: Industrial Valorization of Pyrolysis Carbon. In Proceedings of the SPE Europe Energy Conference and Exhibition, Istanbul, Türkiye, 23–25 June 2026; p. Paper SPE-233223-MS. [Google Scholar] [CrossRef]
  8. Musa, T.; Khawaja, R.; Vechot, L.; Elbashir, N. Methane Pyrolysis for Low-Carbon Syngas and Methanol: Economic Viability and Market Constraints. Gases 2026, 6, 18. [Google Scholar] [CrossRef]
  9. Monolith, Inc. Olive Creek Expansion (OCE): Nebraska Made – Critical Materials, town hall handout. Monolith Inc., Lincoln, NE. 25 February 2026. Available online: https://monolith-corp.com/storage/images/photos/town-hall-handouts—overview-2.25.2026.pdf (accessed on 24 October 2026).
  10. Sánchez-Bastardo, N.; Schlögl, R.; Ruland, H. Methane Pyrolysis for Zero-Emission Hydrogen Production: A Potential Bridge Technology from Fossil Fuels to a Renewable and Sustainable Hydrogen Economy. Ind. Eng. Chem. Res. 2021, 60, 11855–11881. [Google Scholar] [CrossRef]
  11. Patlolla, S.R.; Katsu, K.; Sharafian, A.; Wei, K.; Herrera, O.E.; Mérida, W. A Review of Methane Pyrolysis Technologies for Hydrogen Production. Renew. Sustain. Energy Rev. 2023, 181, 113323. [Google Scholar] [CrossRef]
  12. McConnachie, M.; Konarova, M.; Smart, S. Literature Review of the Catalytic Pyrolysis of Methane for Hydrogen and Carbon Production. Int. J. Hydrogen Energy 2023, 48, 25660–25682. [Google Scholar] [CrossRef]
  13. Hantoko, D.; Khan, W.U.; Osman, A.I.; Nasr, M.; Rashwan, A.K.; Gambo, Y.; Al Shoaibi, A.; Chandrasekar, S.; Hossain, M.M. Carbon-Neutral Hydrogen Production by Catalytic Methane Decomposition: A Review. Environ. Chem. Lett. 2024, 22, 1623–1663. [Google Scholar] [CrossRef]
  14. Alhamed, H.; Behar, O.; Saxena, S.; Angikath, F.; Nagaraja, S.; Yousry, A.; Das, R.; Altmann, T.; Dally, B.; Sarathy, S.M. From Methane to Hydrogen: A Comprehensive Review to Assess the Efficiency and Potential of Turquoise Hydrogen Technologies. Int. J. Hydrogen Energy 2024, 68, 635–662. [Google Scholar] [CrossRef]
  15. Portillo, S.B.; Kosari, M.; Li, F. Supported Transition Metals for Catalytic Decomposition of Methane: Advances, Challenges, and Outlook. ACS Catal. 2026, 16, 1784–1801. [Google Scholar] [CrossRef]
  16. Zeza, E.; Pachatouridou, E.; Lappas, A.A.; Iliopoulou, E.F. Cobalt Decarbonization Catalysts Turning Methane to Clean Hydrogen and Valuable Carbon Nanostructures: A Review. Catalysts 2025, 15, 145. [Google Scholar] [CrossRef]
  17. Alves, L.; Pereira, V.; Lagarteira, T.; Mendes, A. Catalytic Methane Decomposition to Boost the Energy Transition: Scientific and Technological Advancements. Renew. Sustain. Energy Rev. 2021, 137, 110465. [Google Scholar] [CrossRef]
  18. Hamdani, I.R.; Ahmad, A.; Chulliyil, H.M.; Srinivasakannan, C.; Shoaibi, A.A.; Hossain, M.M. Thermocatalytic Decomposition of Methane: A Review on Carbon-Based Catalysts. ACS Omega 2023, 8, 28945–28967. [Google Scholar] [CrossRef] [PubMed]
  19. Msheik, M.; Rodat, S.; Abanades, S. Methane Cracking for Hydrogen Production: A Review of Catalytic and Molten Media Pyrolysis. Energies 2021, 14, 3107. [Google Scholar] [CrossRef]
  20. Zhao, L.; Zhu, Y.; Xu, S.; Cao, G.; Duan, H. A Mini-Review on Hydrogen and Carbon Production from Methane Pyrolysis by Molten Media. Energy Fuels 2024, 38, 23175–23191. [Google Scholar] [CrossRef]
  21. Aman Rasidi, N.E.H.; Baharudin, L.; Samsudin, N.A.; Rahmat, N.; Syed-Hassan, S.S.A. Turquoise Hydrogen Energy Production by Methane Pyrolysis in Bubble Column Reactor: A Review of Catalytic Molten Media Formulation and Parametric Optimization. Energy Technol. 2026, 14, e202502219. [Google Scholar] [CrossRef]
  22. Gunarayu, M.R.; Patah, M.F.A.; Wan Daud, W.M.A. Advancements in methane pyrolysis: A comprehensive review of parameters and molten catalysts in bubble column reactors. Renew. Sustain. Energy Rev. 2025, 210, 115197. [Google Scholar] [CrossRef]
  23. Yu, X.; Xu, Q.; Zhu, C.; Cheng, H.; Zou, X.; Lu, X.; Sun, C. Hydrogen Production from Methane Cracking by Molten Catalysts: A Review and New Perspectives. Chemistry 2025, 7, 138. [Google Scholar] [CrossRef]
  24. Baharudin, L. Progress and future direction in turquoise hydrogen production by methane pyrolysis technologies: an overview of solid catalyst, plasma, plasma–catalyst hybrid, and molten media catalyst systems. Fuel 2025, 401, 135837. [Google Scholar] [CrossRef]
  25. Lotfollahzade Moghaddam, A.; Hejazi, S.; Fattahi, M.; Kibria, M.G.; Thomson, M.J.; AlEisa, R.; Khan, M.A. Methane pyrolysis for hydrogen production: navigating the path to a net zero future. Energy Environ. Sci. 2025, 18, 2747–2790. [Google Scholar] [CrossRef]
  26. Prabowo, J.; Lai, L.; Chivers, B.; Burke, D.; Dinh, A.H.; Ye, L.; Wang, Y.; Wang, Y.; Wei, L.; Chen, Y. Solid carbon co-products from hydrogen production by methane pyrolysis: Current understandings and recent progress. Carbon 2024, 216, 118507. [Google Scholar] [CrossRef]
  27. Zhang, Y.; Dutta, S.; Xu, Z.; Alessi, D.S.; Maboudian, R.; Gadikota, G.; Tsang, D.C.W. Valorizing carbon black byproducts from methane pyrolysis. Chem. Circ. 2026, 1, 100082. [Google Scholar] [CrossRef]
  28. Weber, R.S.; Xu, M.; Lopez-Ruiz, J.A.; Jiang, C.; Hu, J.; Dagle, R.A. Toward Rational Design of Nickel Catalysts for Thermocatalytic Decomposition of Methane for Carbon Dioxide-Free Hydrogen and Value-Added Carbon Co-Product: A Review. ChemCatChem 2024, 16, e202301629. [Google Scholar] [CrossRef]
  29. Ba-Tuq, A.S.; Alhamidi, A.; Rawat, A.; Hossain, M.M. Catalytic methane decomposition as a route to CO2-free hydrogen: A review on kinetics, and reactor design. Chem. Eng. Res. Des. 2026, 230, 337–365. [Google Scholar] [CrossRef]
  30. Page, M.J.; McKenzie, J.E.; Bossuyt, P.M.; Boutron, I.; Hoffmann, T.C.; Mulrow, C.D.; Shamseer, L.; Tetzlaff, J.M.; Akl, E.A.; Brennan, S.E.; et al. The PRISMA 2020 Statement: An Updated Guideline for Reporting Systematic Reviews. BMJ 2021, 372, n71. [Google Scholar] [CrossRef] [PubMed]
  31. Rethlefsen, M.L.; Kirtley, S.; Waffenschmidt, S.; Ayala, A.P.; Moher, D.; Page, M.J.; Koffel, J.B.; PRISMA-S Group. PRISMA-S: An Extension to the PRISMA Statement for Reporting Literature Searches in Systematic Reviews. Syst. Rev. 2021, 10, 39. [Google Scholar] [CrossRef]
  32. Lee, Y.-P.; Chang, C.-W.; Lin, Y.-C.; Luo, C.-S.; Wu, S.-L.; Ou, M.-N.; Kuo, H.-P.; Lee, C.-H.; Chen, Y.-G.; Liao, J.C.; et al. Methane pyrolysis for mixed hydrogen power generation: Performance of two pilot-scale moving-beds. Int. J. Hydrogen Energy 2025, 193, 152408. [Google Scholar] [CrossRef]
  33. Alhamed, H.; Behar, O.; Baaqel, H.; Nagaraja, S.S.; Alghamdi, Z.; Sarathy, S.M. Prioritizing Technologies for Low-Carbon Hydrogen Production under Technical and Market Uncertainty. Appl. Energy 2026, 414, 127827. [Google Scholar] [CrossRef]
  34. d’Entremont, S.; Miederhoff, N.; Buraimoh, M.; Bi, X.; Upham, D.C. Dynamic Molten Cu–In Droplets Catalyze Selective Synthesis of Multi-Walled Carbon Nanotubes During Methane Pyrolysis. ChemCatChem 2025, 17, e01125. [Google Scholar] [CrossRef]
  35. Łamacz, A.; Łabojko, G. CNT and H2 Production during CH4 Decomposition over Ni/CeZrO2. II. Catalyst Performance and Its Regeneration in a Fluidized Bed. ChemEngineering 2019, 3, 25. [Google Scholar] [CrossRef]
  36. Kutteri, D.A.; Wang, I.-W.; Samanta, A.; Li, L.; Hu, J. Methane decomposition to tip and base grown carbon nanotubes and COx-free H2 over mono- and bimetallic 3d transition metal catalysts. Catal. Sci. Technol. 2018, 8, 858–869. [Google Scholar] [CrossRef]
  37. Alturki, H.S.; Alterary, S.S.; Abahussain, A.A.M.; Osman, A.I.; Bayazed, M.O.; Ibrahim, A.A.; Alarifi, N.; Almubaddel, F.S.; Saeed, A.M.M.; Kumar, R.; et al. Iron-Based Catalysts on Tailored Alumina Supports for COx-Free Methane Decomposition to H2 and Carbon. ChemistryOpen 2026, 15, e70282. [Google Scholar] [CrossRef] [PubMed]
  38. Mohapatra, G.; Lee, Y.J.; Seo, H. Sub-valent copper-promoted nickel-bismuth alloy for enhanced methane conversion and high-quality carbon recovery during methane pyrolysis. Chem. Eng. J. 2026, 547, 180839. [Google Scholar] [CrossRef]
  39. Gigantino, M.; Moise, H.; Haribal, V.; Tong, A.; Shen, J.P.; Saad, D.; Fishman, J.; Nelson, A.; Voorhis, H.; Sun, E.; et al. Oxidant-assisted methane pyrolysis. Chem. Sci. 2025, 16, 13256–13266. [Google Scholar] [CrossRef] [PubMed]
  40. Wu, C.-W.; Law, Z.X.; Zeng, Y.-C.; Lin, K.-H.; Tsai, D.-H. Chemical looping of catalytic methane decomposition with reverse Boudouard reaction using dual functional Ni-FeOx nanoparticle cluster for CO2-negative H2 production. Chem. Eng. J. 2025, 511, 162067. [Google Scholar] [CrossRef]
  41. Ahmed, H.; BaQais, A.; Ali, F.A.A.; Osman, A.I.; Fakeeha, A.H.; Abasaeed, A.E.; Ibrahim, A.A.; Adil, S.F.; Algarni, T.S.; Al-Fatesh, A.S. Revolutionizing Hydrogen Production: Unveiling the Role of Liquid Metals in Methane Pyrolysis over Iron Catalysts Supported on Titanium Dioxide and Alumina. Catalysts 2025, 15, 631. [Google Scholar] [CrossRef]
  42. Jun, U.; Ku, B.-J.; Gwon, Y.; Kim, D.-H.; Kim, M.; Jeon, I.-J.; Lee, H.; Shim, J.-O.; Lee, K. Influence of Metal Composition and Support Material on Carbon Yield and Quality in the Direct Decomposition of Methane. Molecules 2025, 30, 1903. [Google Scholar] [CrossRef] [PubMed]
  43. Alves, L.; Pereira, V.; Delgado, S.; Atashi, N.; Dias, P.; Lagarteira, T.; Prieto, G.; Mendes, A. Regeneration of methane splitting catalysts by interfacial hydrogenation. Chem. Eng. J. 2024, 500, 157046. [Google Scholar] [CrossRef]
  44. Sun, E.; Zhai, S.; Kim, D.; Gigantino, M.; Haribal, V.; Dewey, O.S.; Williams, S.M.; Wan, G.; Nelson, A.; Marin-Quiros, S.; et al. A semi-continuous process for co-production of CO2-free hydrogen and carbon nanotubes via methane pyrolysis. Cell Rep. Phys. Sci. 2023, 4, 101338. [Google Scholar] [CrossRef]
  45. Yahyazadeh, A.; Di Liddo, L.; Sui, R.; Marriott, R.; Thomson, M.J. Production of high yield carbon nanotubes and COx-free hydrogen using nickel-based catalyst through microwave-driven methane pyrolysis. Carbon Trends 2026, 24, 100681. [Google Scholar] [CrossRef]
  46. Tian, Q.; Zhao, D.; Ma, X.; Ma, Z. Corncob char-supported iron catalyst for hydrogen production via methane pyrolysis with carbon-iron co-utilization for steelmaking. Fuel 2027, 430, 141124. [Google Scholar] [CrossRef]
  47. Zhang, L.; Zhang, W.; Poh, C.K.; He, H.; Kouk, Q.Y.; Ding, O.L.; Zhang, L.; Chan, S.H.; Zeng, J.; Cao, G.; et al. Catalytic decomposition of methane: Ni-promoted perovskite oxide catalysts for turquoise hydrogen and carbon nanomaterials Co-production. Energy Mater. 2025, 5, 500023. [Google Scholar] [CrossRef]
  48. Liu, M.; Huang, Z.; Zhou, Y.; Zhan, J.; Zhang, K.; Yang, M.; Zhou, Y. Optimized Process for Melt Pyrolysis of Methane to Produce Hydrogen and Carbon Black over Ni Foam/NaCl-KCl Catalyst. Processes 2023, 11, 360. [Google Scholar] [CrossRef]
  49. Takenaka, S.; Tomikubo, Y.; Kato, E.; Otsuka, K. Sequential production of H2 and CO over supported Ni catalysts. Fuel 2004, 83, 47–57. [Google Scholar] [CrossRef]
  50. Li, X.; Zhao, S.; Deng, C.; Chen, R.; Xie, F.; Wu, Z.; Ma, Z.-F.; Weng, G.-M. Cost-effective hydrotalcite-derived Fe-based catalysts for stable and continuous catalytic methane decomposition. J. Mater. Chem. A 2026, 14, 1866–1883. [Google Scholar] [CrossRef]
  51. Wang, M.; Hui, Y.; He, D.; Yan, X.; Zhang, R.; Guo, S.; Li, M.; Qiu, Y.; Zhao, P.; Bhattacharya, S.; et al. Carbon nanotube formation via catalytic methane pyrolysis over molten NiMoCu-Bi catalysts. Fuel 2027, 431, 141938. [Google Scholar] [CrossRef]
  52. Qian, J.X.; Enakonda, L.R.; Wang, W.J.; Gary, D.; Del-Gallo, P.; Basset, J.-M.; Liu, D.B.; Zhou, L. Optimization of a fluidized bed reactor for methane decomposition over Fe/Al2O3 catalysts: Activity and regeneration studies. Int. J. Hydrogen Energy 2019, 44, 31700–31711. [Google Scholar] [CrossRef]
  53. Kim, J.; Oh, C.; Oh, H.; Lee, Y.; Seo, H.; Kim, Y.K. Catalytic methane pyrolysis for simultaneous production of hydrogen and graphitic carbon using a ceramic sparger in a molten NiSn alloy. Carbon 2023, 207, 1–12. [Google Scholar] [CrossRef]
  54. Helveg, S.; López-Cartes, C.; Sehested, J.; Hansen, P.L.; Clausen, B.S.; Rostrup-Nielsen, J.R.; Abild-Pedersen, F.; Nørskov, J.K. Atomic-scale imaging of carbon nanofibre growth. Nature 2004, 427, 426–429. [Google Scholar] [CrossRef] [PubMed]
  55. Chen, L.; Noreña, L.E.; Wang, J.A.; Limas, R.; Arellano, U.; Vargas, O.A.G. Promoting Role of Amorphous Carbon and Carbon Nanotubes Growth Modes of Methane Decomposition in One-Pot Catalytic Approach. Catalysts 2021, 11, 1217. [Google Scholar] [CrossRef]
  56. Parmar, K.R.; Pant, K.K.; Roy, S. Blue hydrogen and carbon nanotube production via direct catalytic decomposition of methane in fluidized bed reactor: Capture and extraction of carbon in the form of CNTs. Energy Convers. Manag. 2021, 232, 113893. [Google Scholar] [CrossRef]
  57. Liang, W.; Yan, H.; Chen, C.; Lin, D.; Tan, K.; Feng, X.; Liu, Y.; Chen, X.; Yang, C.; Shan, H. Revealing the Effect of Nickel Particle Size on Carbon Formation Type in the Methane Decomposition Reaction. Catalysts 2020, 10, 890. [Google Scholar] [CrossRef]
  58. Fakeeha, A.H.; Barama, S.; Ibrahim, A.A.; Al-Otaibi, R.-L.; Barama, A.; Abasaeed, A.E.; Al-Fatesh, A.S. In Situ Regeneration of Alumina-Supported Cobalt–Iron Catalysts for Hydrogen Production by Catalytic Methane Decomposition. Catalysts 2018, 8, 567. [Google Scholar] [CrossRef]
  59. Su, X.; Liao, J.; Luo, X.; Ouyang, X.; Wei, J.; Gou, F. The Investigation of Methane Pyrolysis and Its Carbon Products Utilizing Molten Metal/Molten Salt Composite Reactors. Processes 2025, 13, 3549. [Google Scholar] [CrossRef]
  60. Xu, M.; Lopez-Ruiz, J.A.; Kovarik, L.; Bowden, M.E.; Davidson, S.D.; Weber, R.S.; Wang, I.-W.; Hu, J.; Dagle, R.A. Structure sensitivity and its effect on methane turnover and carbon co-product selectivity in thermocatalytic decomposition of methane over supported Ni catalysts. Appl. Catal. A Gen. 2021, 611, 117967. [Google Scholar] [CrossRef]
  61. Wang, H.Y.; Ruckenstein, E. Formation of filamentous carbon during methane decomposition over Co–MgO catalysts. Carbon 2002, 40, 1911–1917. [Google Scholar] [CrossRef]
  62. Shah, M.; Al Mesfer, M.K.; Danish, M. Facile synthesis of Co-Rh bimetallic catalysts for methane decomposition: Effect of support morphology. Fuel 2022, 330, 125596. [Google Scholar] [CrossRef]
  63. Al Alwan, B.A.; Shah, M.; Danish, M.; Al Mesfer, M.K.; Khan, M.I.; Natarajan, V. Enhanced methane decomposition over transition metal-based tri-metallic catalysts for the production of COx free hydrogen. J. Indian Chem. Soc. 2022, 99, 100393. [Google Scholar] [CrossRef]
  64. Al Mesfer, M.K.; Danish, M.; Shah, M. Synthesis, evaluation, and kinetic assessment of Co-based catalyst for enhanced methane decomposition reaction for hydrogen production. Int. J. Chem. Kinet. 2022, 54, 90–103. [Google Scholar] [CrossRef]
  65. Shah, M.; Bordoloi, A.; Nayak, A.K.; Mondal, P. Effect of Ti/Al ratio on the performance of Ni/TiO2-Al2O3 catalyst for methane reforming with CO2. Fuel Process. Technol. 2019, 192, 21–35. [Google Scholar] [CrossRef]
  66. Shah, M.; Al Mesfer, M.K.; Danish, M. Effect of titania synthesis conditions on the catalytic performance of mesoporous Ni/TiO2 catalysts for carbon dioxide reforming of methane. Int. J. Hydrogen Energy 2022, 47, 8867–8874. [Google Scholar] [CrossRef]
  67. Shah, M.; Das, T.; Mondal, P. Development of nanocrystalline mesoporous Pt promoted Co-based catalysts for carbon dioxide reforming of methane. Fuel 2022, 313, 122683. [Google Scholar] [CrossRef]
  68. Al Mesfer, M.K.; Das, S.; Shah, M.; Danish, M. Design of Ru-Co/MgO-Al2O3 catalyst system for CO2 reforming of methane: Performance investigation concerning the Mg/Al ratio. J. Ind. Eng. Chem. 2024, 130, 468–482. [Google Scholar] [CrossRef]
  69. Shah, M.; Das, S.; Nayak, A.K.; Mondal, P.; Bordoloi, A. Smart designing of metal-support interface for imperishable dry reforming catalyst. Appl. Catal. A Gen. 2018, 556, 137–154. [Google Scholar] [CrossRef]
  70. Das, S.; Sengupta, M.; Bag, A.; Shah, M.; Bordoloi, A. Facile synthesis of highly disperse Ni–Co nanoparticles over mesoporous silica for enhanced methane dry reforming. Nanoscale 2018, 10, 6409–6425. [Google Scholar] [CrossRef] [PubMed]
  71. Shah, M.; Bordoloi, A.; Nayak, A.K.; Mondal, P. Experimental and Kinetic Studies of Methane Reforming with CO2 over a La-Doped Ni/Al2O3 Bimodal Catalyst. Ind. Eng. Chem. Res. 2021, 60, 18243–18255. [Google Scholar] [CrossRef]
  72. Shah, M.; Das, S.; Mondal, P.; Al Mesfer, M.K.; Danish, M.; Ansari, K.B.; Diab, M.A.; Kim, Y. Design of bi-metallic Ni-Pt supported over mesoporous titania catalysts: Role of bimodal porosity and mixed anatase-rutile phases in low-temperature partial oxidation of methane. J. Taiwan Inst. Chem. Eng. 2026, 188, 106810. [Google Scholar] [CrossRef]
  73. Shah, M.; Al Mesfer, M.K.; Danish, M. Design and optimization of Ni–Fe–La based catalytic system for CO2 utilization for sustainable syngas production via dry reforming of methane. J. Energy Inst. 2023, 110, 101346. [Google Scholar] [CrossRef]
  74. Shah, M.; Al Mesfer, M.K.; Danish, M.; Mondal, P.; Goyal, H.; Das, S. Study on the effect of promotors in CO2 utilization for syngas production via dry reforming of methane over Co-MOX/TiO2-Al2O3 (MOX = La, Ce, Mg, and K) catalysts. Fuel Process. Technol. 2024, 257, 108089. [Google Scholar] [CrossRef]
  75. Shah, M. Development of versatile Ni–Ce-based catalyst for syngas production through dry reforming and catalytic partial oxidation of methane. Int. J. Hydrogen Energy 2025, 105, 505–520. [Google Scholar] [CrossRef]
  76. Takenaka, S.; Shigeta, Y.; Tanabe, E.; Otsuka, K. Methane Decomposition into Hydrogen and Carbon Nanofibers over Supported Pd−Ni Catalysts: Characterization of the Catalysts during the Reaction. J. Phys. Chem. B 2004, 108, 7656–7664. [Google Scholar] [CrossRef]
  77. Li, Y.; Chen, J.; Qin, Y.; Chang, L. Simultaneous Production of Hydrogen and Nanocarbon from Decomposition of Methane on a Nickel-Based Catalyst. Energy Fuels 2000, 14, 1188–1194. [Google Scholar] [CrossRef]
  78. Torres, D.; Pinilla, J.L.; Suelves, I. Co-, Cu- and Fe-Doped Ni/Al2O3 Catalysts for the Catalytic Decomposition of Methane into Hydrogen and Carbon Nanofibers. Catalysts 2018, 8, 300. [Google Scholar] [CrossRef]
  79. Al Mesfer, M.K.; Danish, M.; Shah, M. Synthesis and optimization of hydrotalcite derived Ni-Fe-Cu based catalysts for catalytic methane decomposition process using the design of experiment approach. J. Taiwan Inst. Chem. Eng. 2021, 128, 370–379. [Google Scholar] [CrossRef]
  80. Chai, S.-P.; Lee, K.-Y.; Ichikawa, S.; Mohamed, A.R. Synthesis of carbon nanotubes by methane decomposition over Co–Mo/Al2O3: Process study and optimization using response surface methodology. Appl. Catal. A Gen. 2011, 396, 52–58. [Google Scholar] [CrossRef]
  81. Han, S.B.; Kim, M.S.; Deng, Y.; Kang, K.Y.; Choi, J.-S.; Jang, E.; Bae, J.W. Chemical looping-based catalytic CH4 decomposition and successive coke gasification with CO2 on ordered mesoporous NiMCeOx (M = Co, Zr, La). Chem. Eng. J. 2024, 489, 151034. [Google Scholar] [CrossRef]
  82. Soliman, A.M.S.; Tschentscher, R.; Akporiaye, D.; Al-Rawashdeh, M. Effect of Ni/SiO2 catalyst preparation method on methane decomposition and CO2 gasification cycles. Fuel 2024, 368, 131585. [Google Scholar] [CrossRef]
  83. Rahimi, N.; Kang, D.; Gelinas, J.; Menon, A.; Gordon, M.J.; Metiu, H.; McFarland, E.W. Solid carbon production and recovery from high temperature methane pyrolysis in bubble columns containing molten metals and molten salts. Carbon 2019, 151, 181–191. [Google Scholar] [CrossRef]
  84. Msheik, M.; Rodat, S.; Abanades, S. Enhancing molten tin methane pyrolysis performance for hydrogen and carbon production in a hybrid solar/electric bubbling reactor. Int. J. Hydrogen Energy 2024, 49, 962–980. [Google Scholar] [CrossRef]
  85. Ji, Y.; Palmer, C.; Foley, E.E.; Giovine, R.; Yoshida, E.; Sebti, E.; Patterson, A.R.; McFarland, E.; Clément, R.J. Valorizing the carbon byproduct of methane pyrolysis in batteries. Carbon 2023, 204, 26–35. [Google Scholar] [CrossRef]
  86. Boo, J.; Ko, E.H.; Park, N.-K.; Ryu, C.; Kim, Y.-H.; Park, J.; Kang, D. Methane Pyrolysis in Molten Potassium Chloride: An Experimental and Economic Analysis. Energies 2021, 14, 8182. [Google Scholar] [CrossRef]
  87. Kang, D.; Palmer, C.; Mannini, D.; Rahimi, N.; Gordon, M.J.; Metiu, H.; McFarland, E.W. Catalytic Methane Pyrolysis in Molten Alkali Chloride Salts Containing Iron. ACS Catal. 2020, 10, 7032–7042. [Google Scholar] [CrossRef]
  88. Kang, H.; Lee, Y.H.; Ko, H.Y.; Oh, J.-H.; Choi, S. Effect of post-treatments on the performance of carbon black derived from plasma methane pyrolysis as a battery conductive agent. Int. J. Hydrogen Energy 2025, 141, 1029–1038. [Google Scholar] [CrossRef]
  89. Pérez, B.J.L.; Jiménez, J.A.M.; Bhardwaj, R.; Goetheer, E.; van Sint Annaland, M.; Gallucci, F. Methane pyrolysis in a molten gallium bubble column reactor for sustainable hydrogen production: Proof of concept & techno-economic assessment. Int. J. Hydrogen Energy 2021, 46, 4917–4935. [Google Scholar] [CrossRef]
  90. Yang, M.; Baeyens, J.; Li, S.; Zhang, H. Hydrogen and carbon produced by fluidized bed catalytic methane decomposition. Chem. Eng. Res. Des. 2024, 204, 67–80. [Google Scholar] [CrossRef]
  91. Alcázar, H.E.; Chire, E.; Vargas, M.M.; Villagarcía, B.L.; Neira, J.; Contin, A.; Alcázar, L.O. Production and characterization of carbon nanotubes by methane decomposition over Ni–Fe/Al2O3 catalyst and its application as nanofillers in polypropylene matrix. Mater. Res. Express 2021, 8, 115001. [Google Scholar] [CrossRef]
  92. Oliveira, H.A.; Franceschini, D.F.; Passos, F.B. Cobalt Catalyst Characterization for Methane Decomposition and Carbon Nanotube Growth. J. Braz. Chem. Soc. 2014, 25, 2339–2349. [Google Scholar] [CrossRef]
  93. Moise, H.; Moll, S.; Pathak, S.; Martinez-Navarro, J.; Varanasi, S.; Xu, K.; McFarland, E.; Majumdar, A.; Cargnello, M. Autothermal Methane Pyrolysis: Scalable Heat Integration for Hydrogen and Graphite Production. Science 2026, 393, 1014–1020. [Google Scholar] [CrossRef] [PubMed]
  94. Zhang, Y.; Smith, K.J. Carbon Formation Thresholds and Catalyst Deactivation During CH4 Decomposition on Supported Co and Ni Catalysts. Catal. Lett. 2004, 95, 7–12. [Google Scholar] [CrossRef]
  95. Avdeeva, L.B.; Kochubey, D.I.; Shaikhutdinov, S.K. Cobalt catalysts of methane decomposition: accumulation of the filamentous carbon. Appl. Catal. A Gen. 1999, 177, 43–51. [Google Scholar] [CrossRef]
  96. Lopez-Ruiz, J.A.; Jiang, Y.; Riedel, N.W.; Weber, R.S.; Jiang, C.; Xu, M.; Hu, J.; Dagle, R.A. CO2-free (turquoise) H2 at $1/kg via thermocatalytic decomposition of methane and sale of solid carbon co-product. An experimental and techno-economic analysis. Int. J. Hydrogen Energy 2026, 207, 153492. [Google Scholar] [CrossRef]
  97. Nikolis, D.; Raman, S.; Pyl, S.; Hellgardt, K. Abrasion-assisted methane pyrolysis in a bubbling fluidized bed using low-surface-area carbon-sphere–supported Fe/Co/Ni catalysts that shed pyrolytic carbon. Chem. Eng. J. 2026, 540, 177055. [Google Scholar] [CrossRef]
  98. Chu, Z.; Zhang, J.; Zhao, W.; Yang, Y.; Zhao, J.; Li, Y. H2 and carbon production from CH4 decomposition and regeneration based on Fe/CaO-Ca12Al14O33 catalyst looping cycles. Chem. Eng. J. 2024, 497, 154599. [Google Scholar] [CrossRef]
  99. Becker, T.; Richter, M.; Agar, D.W. Methane pyrolysis: Kinetic studies and mechanical removal of carbon deposits in reactors of different materials. Int. J. Hydrogen Energy 2023, 48, 2112–2129. [Google Scholar] [CrossRef]
  100. Yao, Y.; Pan, Y.; Lai, L.; Yu, Z.; Chen, J.; Yu, Y.; Darma, T.; Tao, Y.; Cao, L.; Chivers, B.; et al. Carbon/iron co-product from clean hydrogen production as a tri-functional adsorbent and catalyst for efficient wastewater treatment. Appl. Catal. B Environ. 2024, 342, 123380. [Google Scholar] [CrossRef]
  101. Pan, Y.; Lo, V.; Cao, L.; Roy, A.; Chivers, B.; Noorbehesht, N.; Yao, Y.; Wang, J.; Wei, L.; Chen, Y. Graphitic carbon from catalytic methane decomposition as efficient conductive additives for zinc-carbon batteries. Carbon 2022, 192, 84–92. [Google Scholar] [CrossRef]
  102. Hofberger, C.; Dietrich, B.; Krumholz, R.; Noglik, A.P.; Olbricht, M.; Schatzmann, S.; Stoppel, L.; Richter, M.; Uhlenbruck, N.; Wetzel, T. Technical Aspects of Natural Gas Pyrolysis in Liquid Metal Bubble Column Reactors. Energy Technol. 2024, 12, 2400183. [Google Scholar] [CrossRef]
  103. Cooper-Baldock, Z.; De La Perrelle, T.; Phelps, C.; Russell, M.; Ryan, L.; Schofield, J.; Nathan, G.J.; Jafarian, M. Preliminary Evaluation of Methods for Continuous Carbon Removal from a Molten Catalyst Bubbling Methane Pyrolysis Reactor. Energies 2024, 17, 290. [Google Scholar] [CrossRef]
  104. Mortazavi, S.; Novinrooz, A.; Reyhani, A.; Mirershadi, S. Effects of acid treatment duration and sulfuric acid molarity on purification of multi-walled carbon nanotubes. Open Phys. 2010, 8, 940–946. [Google Scholar] [CrossRef]
  105. Kang, H.; Oh, J.-H.; Lee, Y.H.; Yang, S.; Choi, S. Study on the Value-Added Carbon Products from Methane Pyrolysis with the Thermal Plasma Process. Appl. Sci. Converg. Technol. 2024, 33, 13–17. [Google Scholar] [CrossRef]
  106. Sun, J.; Tu, R.; Xu, Y.; Yang, H.; Yu, T.; Zhai, D.; Ci, X.; Deng, W. Machine learning aided design of single-atom alloy catalysts for methane cracking. Nat. Commun. 2024, 15, 6036. [Google Scholar] [CrossRef] [PubMed]
  107. Hatanaka, T.; Yoda, Y. Use of a swirling flow to mechanically regenerate catalysts after methane decomposition. Int. J. Hydrogen Energy 2022, 47, 20176–20184. [Google Scholar] [CrossRef]
  108. Pham, D.A.; Go, K.-S.; Kim, W.; Lee, D.H.; Ryu, H.-J.; Nho, N.S. Numerical investigation of segregation behavior in a fluidized bed reactor for high-purity carbon production via catalytic methane decomposition. Energy Convers. Manag. 2025, 346, 120412. [Google Scholar] [CrossRef]
  109. Keller, M.; Sharma, A. Hydrogen Production via Methane Cracking on Dry-Coated Fe/ZrO2with Support Recycle in a Fluidized Bed Process. Energy Fuels 2021, 35, 847–855. [Google Scholar] [CrossRef]
  110. Dawkins, M.; Saal, D.; Marco, J.F.; Reynolds, J.; Dann, S. An iron ore-based catalyst for producing hydrogen and metallurgical carbon via catalytic methane pyrolysis for decarbonisation of the steel industry. Int. J. Hydrogen Energy 2023, 48, 21765–21777. [Google Scholar] [CrossRef]
  111. Edwards, E.R.; Antunes, E.F.; Botelho, E.C.; Baldan, M.R.; Corat, E.J. Evaluation of residual iron in carbon nanotubes purified by acid treatments. Appl. Surf. Sci. 2011, 258, 641–648. [Google Scholar] [CrossRef]
  112. Ko, D.H.; Kang, S.C.; Lee, C.W.; Im, J.S. Effects of support porosity of Co-Mo/MgO catalyst on methane catalytic decomposition for carbon and hydrogen production. J. Ind. Eng. Chem. 2022, 112, 162–170. [Google Scholar] [CrossRef]
  113. Luo, X.; Cao, Z.; Wang, S.; Ye, Z.; Wei, J.; Yang, B.; Gou, F. Copper-tin catalyzed methane pyrolysis and solid carbon products as anode materials for sodium-ion batteries. Int. J. Green Energy 2025, 22, 2597–2609. [Google Scholar] [CrossRef]
  114. Prabowo, J.; Pan, Y.; Zheng, Z.; Lai, L.; Yang, X.; She, F.; Chen, J.; Liu, F.; Chivers, B.; Wei, L.; et al. Dual-functional graphitic carbon materials from methane pyrolysis for lithium-ion batteries. Carbon 2025, 234, 120038. [Google Scholar] [CrossRef]
  115. Pan, Y.; Cao, L.; Yao, Y.; Tao, Y.; Lo, V.; Zheng, Z.; Chivers, B.; Prabowo, J.; Liu, F.; Lai, L.; et al. Graphitic Co-Products of Clean Hydrogen Production Enabling High-Rate-Performance Dual-Carbon Batteries. Adv. Energy Mater. 2023, 13, 2300495. [Google Scholar] [CrossRef]
  116. Upham, D.C.; Agarwal, V.; Khechfe, A.; Snodgrass, Z.R.; Gordon, M.J.; Metiu, H.; McFarland, E.W. Catalytic molten metals for the direct conversion of methane to hydrogen and separable carbon. Science 2017, 358, 917–921. [Google Scholar] [CrossRef] [PubMed]
  117. Kang, D.; Rahimi, N.; Gordon, M.J.; Metiu, H.; McFarland, E.W. Catalytic methane pyrolysis in molten MnCl2-KCl. Appl. Catal. B Environ. 2019, 254, 659–666. [Google Scholar] [CrossRef]
  118. Msheik, M.; Rodat, S.; Abanades, S. Solar methane pyrolysis in a liquid metal bubble column reactor: Effect of medium type and gas injection configuration. J. Anal. Appl. Pyrolysis 2024, 183, 106756. [Google Scholar] [CrossRef]
  119. Cai, G.; Miederhoff, N.; d’Entremont, S.; Feigl, K.; Pfeiffer, M.; Popp, S.; Upham, D.C. Production of Carbon Fibers Using a Molten Cu–In Catalyst for Methane Pyrolysis. ACS Appl. Mater. Interfaces 2024, 16, 67674–67682. [Google Scholar] [CrossRef] [PubMed]
  120. Parkinson, B.; Patzschke, C.F.; Nikolis, D.; Raman, S.; Dankworth, D.C.; Hellgardt, K. Methane pyrolysis in monovalent alkali halide salts: Kinetics and pyrolytic carbon properties. Int. J. Hydrogen Energy 2021, 46, 6225–6238. [Google Scholar] [CrossRef]
  121. Seo, J.-C.; Park, S.; Park, G.; Lee, Y.; Han, S.J.; Kim, S.K. Catalytic CH4 pyrolysis promoted by the interface of a molten metal–salt hybrid system. Gas. Sci. Eng. 2023, 115, 205017. [Google Scholar] [CrossRef]
  122. Aster, P.; Scheiblehner, D.; Leuchtenmüller, M.; Tunes, M.A.; Berger, T.; Pichler, I.; Rameshan, C.; Antrekowitsch, J. Multiscale carbon characterization obtained from methane pyrolysis in a pilot-scale molten metal reactor. Int. J. Hydrogen Energy 2026, 289, 158317. [Google Scholar] [CrossRef]
  123. Zaghloul, N.; Kodama, S.; Sekiguchi, H. Hydrogen Production by Methane Pyrolysis in a Molten-Metal Bubble Column. Chem. Eng. Technol. 2021, 44, 1986–1993. [Google Scholar] [CrossRef]
  124. Yang, S.-B.; Lee, Y.H.; Choi, S.; Oh, J.-H. Post-treatment of solid carbon by-products from plasma methane pyrolysis: Removal of polycyclic aromatic hydrocarbons and improvement of structure properties. Powder Technol. 2026, 478, 122481. [Google Scholar] [CrossRef]
  125. Wang, F.; Wang, F.; Hong, R.; Lv, X.; Zheng, Y. High-purity few-layer graphene from plasma pyrolysis of methane as conductive additive for LiFePO4 lithium ion battery. J. Mater. Res. Technol. 2020, 9, 10004–10015. [Google Scholar] [CrossRef]
  126. Argyle, M.; Bartholomew, C. Heterogeneous Catalyst Deactivation and Regeneration: A Review. Catalysts 2015, 5, 145–269. [Google Scholar] [CrossRef]
  127. Chu, Z.; Zhao, W.; Xu, D.; Liu, W.; Han, K.; He, Z.; Li, Y. The catalytic decomposition of CH4 using Ce-doped Fe/CaO-Ca12Al14O33 catalyst and its regeneration performance for H2 production. Sep. Purif. Technol. 2025, 355, 129670. [Google Scholar] [CrossRef]
  128. Chu, Z.W.; Li, Y.J.; Zhao, W.H.; Zhou, Z.Z.; Fang, Y.; Han, K.H.; Liu, F.; Yang, L. H2 production performance in CH4 decomposition/regeneration cycles using Fe/CaO-based solid waste material as a catalyst with perovskite structure. Sep. Purif. Technol. 2025, 368. [Google Scholar] [CrossRef]
  129. Chu, Z.; Zhang, W.; Zhao, W.; Xu, D.; He, Z.; Han, K.; Li, Y. CH4 decomposition using catalyst pellets prepared from red mud and calcium carbide slag under fluidization for the production of H2 and carbon-based anode materials. Fuel 2026, 407, 137282. [Google Scholar] [CrossRef]
  130. Jiao, F.; Yang, S.; Weng, Y.; Mei, L.; Shi, X.; Yu, H.; Liu, Q. Solar methane carbon cyclic reforming with over 40% solar-to-fuel efficiency and nearly 100% selectivity in kWth scale solar fuel production prototype. Chem. Eng. J. 2025, 512, 162435. [Google Scholar] [CrossRef]
  131. Amin, A.M.; Croiset, E.; Malaibari, Z.; Epling, W. Hydrogen production by methane cracking using Ni-supported catalysts in a fluidized bed. Int. J. Hydrogen Energy 2012, 37, 10690–10701. [Google Scholar] [CrossRef]
  132. Ahmed, H.; Fakeeha, A.H.; Al-Alweet, F.M.; Abasaeed, A.E.; Ibrahim, A.A.; Kumar, R.; Saeed, A.M.M.; Al-Fatesh, A.S. Methane Decomposition over a Titanium-Alumina and Iron Catalyst Assisted by Lanthanides to Produce High-Performance COx-Free H2 and Carbon Nanotubes. Catalysts 2025, 15, 77. [Google Scholar] [CrossRef]
  133. Varnagiris, Š.; Urbonavičius, M.; Tučkutė, S.; Nair, V.R.; Knoks, A.; Grinberga, L.; Sika, R.K.; Kmet, B.; Kuscer, D. Investigation of Coked Catalyst Regeneration via Non-Thermal Plasma Treatment and Its Reuse for Hydrogen Production from Methane Pyrolysis. Molecules 2026, 31, 1733. [Google Scholar] [CrossRef] [PubMed]
  134. de Cataldo, A.; Colbertaldo, P.; Beretta, A.; Groppi, G.; Pinilla, J.L.; Suelves, I.; Campanari, S.; Romano, M.C. Blueish hydrogen production via methane pyrolysis and remote CO2 capture and storage. Int. J. Hydrogen Energy 2025, 146, 149723. [Google Scholar] [CrossRef]
  135. Olisa, E.; Pelucchi, S.; De Tommaso, J.; Longhi, M.; Galli, F. Carbon-catalyzed methane pyrolysis I: Experimental data and modeling of deactivation towards the measurement of intrinsic kinetic constant. Chem. Eng. J. 2026, 548, 181578. [Google Scholar] [CrossRef]
  136. Mokashi, M.; Shirsath, A.B.; Çelik, A.; Lott, P.; Müller, H.; Tischer, S.; Maier, L.; Bode, J.; Schlereth, D.; Scheiff, F.; et al. Methane pyrolysis in packed bed reactors: Kinetic modeling, numerical simulations, and experimental insights. Chem. Eng. J. 2024, 485, 149684. [Google Scholar] [CrossRef]
  137. Pereira, V.; Alves, L.; Dias, P.; Lagarteira, T.; Mendes, A. Low-temperature catalytic methane splitting: A new reactor design for long-term hydrogen production. Fuel 2025, 396, 135316. [Google Scholar] [CrossRef]
  138. Lott, P.; Mokashi, M.B.; Müller, H.; Heitlinger, D.J.; Lichtenberg, S.; Shirsath, A.B.; Janzer, C.; Tischer, S.; Maier, L.; Deutschmann, O. Hydrogen Production and Carbon Capture by Gas-Phase Methane Pyrolysis: A Feasibility Study. ChemSusChem 2023, 16, e202201720. [Google Scholar] [CrossRef] [PubMed]
  139. Abbas, H.F.; Ashik, U.P.M.; Mohammed, S.A.; Wan Daud, W.M.A. Impact of reactor materials on methane decomposition for hydrogen production. Chem. Eng. Res. Des. 2021, 174, 127–136. [Google Scholar] [CrossRef]
  140. Hadian, M.; Marrevee, D.P.F.; Buist, K.A.; Reesink, B.H.; Bos, A.N.R.; Bavel, A.P.; Kuipers, J.A.M. Kinetic study of thermocatalytic decomposition of methane over nickel supported catalyst in a fluidized bed reactor. Chem. Eng. Sci. 2022, 260, 117938. [Google Scholar] [CrossRef]
  141. Keller, M.; Matsumura, A.; Sharma, A. Spray-dried Fe/Al2O3 as a carbon carrier for COx-free hydrogen production via methane cracking in a fluidized bed process. Chem. Eng. J. 2020, 398, 125612. [Google Scholar] [CrossRef]
  142. Siriwardane, R.; Riley, J.; Atallah, C.; Bobek, M. Investigation of methane and ethane pyrolysis with highly active and durable iron-alumina catalyst to produce hydrogen and valuable nano carbons: Continuous fluidized bed tests and reaction rate analysis. Int. J. Hydrogen Energy 2023, 48, 14210–14225. [Google Scholar] [CrossRef]
  143. Weizhong, Q.; Tang, L.; Zhanwen, W.; Fei, W.; Zhifei, L.; Guohua, L.; Yongdan, L. Production of hydrogen and carbon nanotubes from methane decomposition in a two-stage fluidized bed reactor. Appl. Catal. A Gen. 2004, 260, 223–228. [Google Scholar] [CrossRef]
  144. Hadian, M.; Ramírez, J.G.; de Munck, M.J.A.; Buist, K.A.; Bos, A.N.R.; Kuipers, J.A.M. Comparative analysis of a batch and continuous fluidized bed reactors for thermocatalytic decomposition of methane: A CFD-DEM-MGM approach. Chem. Eng. J. 2024, 484, 149478. [Google Scholar] [CrossRef]
  145. Bae, K.; Kim, D.; Pham, A.D.; Lee, D.; Hwang, B.; Go, K.S.; Kim, W.; Lee, J.K.; Im, J.S.; Kang, S.C.; et al. Simultaneous and Continuous Production of Carbon Nanotubes and Hydrogen by Catalytic CH4 Decomposition in a Pressurized Fluidized-Bed Reactor. Ind. Eng. Chem. Res. 2024, 63, 930–941. [Google Scholar] [CrossRef]
  146. Pinilla, J.L.; de Llobet, S.; Moliner, R.; Suelves, I. H2-rich gases production from Catalytic Decomposition of Biogas: Viability of the process associated to the co-production of carbon nanofibers. Int. J. Hydrogen Energy 2017, 42, 23484–23493. [Google Scholar] [CrossRef]
  147. Hauck, J.A.; Champ, T.A.; Warren, K.J.; Broerman, A.; Wang, B.; Hubler, M.H.; Weimer, A.W. Technoeconomic analysis of the modular valorization of flare gas to carbon additives for concrete. Energy Convers. Manag. 2026, 348, 120783. [Google Scholar] [CrossRef]
  148. Geißler, T.; Abánades, A.; Heinzel, A.; Mehravaran, K.; Müller, G.; Rathnam, R.K.; Rubbia, C.; Salmieri, D.; Stoppel, L.; Stückrad, S.; et al. Hydrogen production via methane pyrolysis in a liquid metal bubble column reactor with a packed bed. Chem. Eng. J. 2016, 299, 192–200. [Google Scholar] [CrossRef]
  149. Hofberger, C.M.; Dietrich, B.; Vera, I.D.; Krumholz, R.; Stoppel, L.; Uhlenbruck, N.; Wetzel, T. Natural Gas Pyrolysis in a Liquid Metal Bubble Column Reaction System—Part I: Experimental Setup and Methods. Hydrogen 2023, 4, 295–306. [Google Scholar] [CrossRef]
  150. Uhlenbruck, N.; Pfeifer, P.; Dietrich, B.; Hofberger, C.M.; Krumholz, R.; Saxler, A.; Schulz, L.; Stoppel, L.; Wetzel, T. A Carbon Capture and Utilization Process for the Production of Solid Carbon Materials from Atmospheric CO2 – Part 1: Process Performance. ChemSusChem 2025, 18, e202401779. [Google Scholar] [CrossRef] [PubMed]
  151. Zong, Z.; Cai, G.; Tabbara, M.; Upham, D.C. CO2-negative fuel production using low-CO2 electricity: Syngas from a combination of methane pyrolysis and dry reforming with techno-economic analysis. Energy Convers. Manag. 2023, 277, 116624. [Google Scholar] [CrossRef]
  152. Zhang, X.; Liu, J.; Li, W.; Zhou, J.; Yang, B.; Xu, C.; Guan, X. Methane Decomposition Enabled by Molten Alkali Chloride Electrolysis. ACS Catal. 2025, 15, 3203–3214. [Google Scholar] [CrossRef]
  153. Pangestu, M.R.G.; Malaibari, Z.; Muhammad, A.; Al-Rowaili, F.N.; Zahid, U. Comprehensive Review on Methane Pyrolysis for Sustainable Hydrogen Production. Energy Fuels 2024, 38, 13514–13538. [Google Scholar] [CrossRef]
  154. Mendes, A. Understanding Catalytic Methane Decomposition: A Swift and Cost-Effective Energy Decarbonization Pathway. Open Access Gov. 2023, 38, 430–431. [Google Scholar] [CrossRef]
  155. Wang, G.; Jin, Y.; Liu, G.; Li, Y. Production of Hydrogen and Nanocarbon from Catalytic Decomposition of Methane over a Ni–Fe/Al2O3 Catalyst. Energy Fuels 2013, 27, 4448–4456. [Google Scholar] [CrossRef]
  156. Chen, L.; Song, Z.; Zhang, S.; Chang, C.-K.; Chuang, Y.-C.; Peng, X.; Dun, C.; Urban, J.J.; Guo, J.; Chen, J.-L.; et al. Ternary NiMo-Bi liquid alloy catalyst for efficient hydrogen production from methane pyrolysis. Science 2023, 381, 857–861. [Google Scholar] [CrossRef] [PubMed]
  157. Geißler, T.; Plevan, M.; Abánades, A.; Heinzel, A.; Mehravaran, K.; Rathnam, R.K.; Rubbia, C.; Salmieri, D.; Stoppel, L.; Stückrad, S.; et al. Experimental investigation and thermo-chemical modeling of methane pyrolysis in a liquid metal bubble column reactor with a packed bed. Int. J. Hydrogen Energy 2015, 40, 14134–14146. [Google Scholar] [CrossRef]
  158. Kim, Y.; Shin, H.; Kim, B.; Kim, G.; Jeong, H.; Im, Y.; Kwak, B.S.; Do, J.Y.; Son, N.; Moon, H.; et al. Methane-pyrolysis-driven interfacial carbon reconstruction for durable high-kinetics silicon anodes with extension to end-of-life photovoltaic silicon. Chem. Eng. J. 2026, 545, 179776. [Google Scholar] [CrossRef]
  159. Peden, J.; Ryley, J.; Terrones, J.; Smail, F.; Elliott, J.A.; Windle, A.; Boies, A. Production of hydrogen and carbon nanotubes from methane using a multi-pass floating catalyst chemical vapour deposition reactor with process gas recycling. Nat. Energy 11 2026, 121–134. [Google Scholar] [CrossRef] [PubMed]
  160. Zhao, D.; Ma, X.; Tian, Q.; Ma, Z. Spent Iron-Char Catalysts Are Not Waste: A Viewpoint on Integrating Methane Pyrolysis with Steelmaking. ACS Sustain. Resour. Manag. 2026, 3, 3274–3281. [Google Scholar] [CrossRef]
  161. Qi, Y.; Jiang, J.; Bao, G.; Sui, H.; Lin, J.; Liu, Y.; Gao, Y. In situ nanocarbon deposition on steel slag via methane pyrolysis for enhanced strength and pore refinement in cement composites. Colloids Surf. A Physicochem. Eng. Asp. 2027, 753, 141925. [Google Scholar] [CrossRef]
  162. Vander Wal, R.; Sengupta, A.; Musselman, E.; Skoptsov, G. Microwave-Driven Plasma-Mediated Methane Cracking: Product Carbon Characterization. C 2018, 4, 61. [Google Scholar] [CrossRef]
  163. Li, J.; Spanu, L.; Heo, J.; Zhang, W.; Gardner, D.W.; Carraro, C.; Maboudian, R.; Monteiro, P.J.M. Sequestration of solid carbon in concrete: A large-scale enabler of lower-carbon intensity hydrogen from natural gas. MRS Bull. 2021, 46, 680–686. [Google Scholar] [CrossRef]
  164. Gao, Y.; Qi, Y.; Bao, G.; Sui, H.; Lin, J.; Miao, J.; Liu, Y. Harnessing methane-derived nanocarbon coatings on steel slag for high-performance cementitious composites. Mater. Today Nano 2026, 35, 100946. [Google Scholar] [CrossRef]
  165. Rubio, M.R.; Martínez, D.J.; Odriozola, J.A.; Centeno, M.Á.; Reyes, F.A.; Laguna, O.H.; Daza, C. Turquoise hydrogen and carbon nanostructures from methane pyrolysis enable a dual approach to clean energy and asphalt enhancement. J. Environ. Chem. Eng. 2026, 14, 121883. [Google Scholar] [CrossRef]
  166. Cao, M.; Li, S.; Wang, S.; Xu, W.; Zhou, X.; Ma, G.; Wang, X.; Nie, L.; Chen, Y. Highly stable hydrotalcite-derived NiCrAl catalyst for methane cracking and directly application for electromagnetic wave absorption. Fuel 2025, 379, 133128. [Google Scholar] [CrossRef]
  167. Li, T.; Wang, C.; Wood, C.A.; Zeng, K.; Dong, Q.; Gonzalez, M.; Jony, B.; Cheng, S.; Zhao, X.; Brozena, A.H.; et al. Methane pyrolysis-enabled production of high-value carbon fibres. Nat. Sustain. 2026, 9, 890–900. [Google Scholar] [CrossRef]
  168. Tsunemi, K. Risk assessment of nano-scale solid carbon sourced from a CO2-free hydrogen manufacturer used at a steel plant and disposed at a landfill site. Process Saf. Environ. Prot. 2023, 170, 1032–1038. [Google Scholar] [CrossRef]
  169. Salas, S.D.; Dunn, J.B. Methane-to-graphite: A pathway to reduce greenhouse gas emissions in the U.S. energy transition. Resour. Conserv. Recycl. 2024, 210, 107832. [Google Scholar] [CrossRef]
  170. Lumbers, B.; Barley, J.; Platte, F. Low-emission hydrogen production via the thermo-catalytic decomposition of methane for the decarbonisation of iron ore mines in Western Australia. Int. J. Hydrogen Energy 2022, 47, 16347–16361. [Google Scholar] [CrossRef]
  171. Tamarona, P.B.; Nijssen, T.M.J.; Vlugt, T.J.H.; Ramdin, M. Techno-economic analysis of catalytic methane pyrolysis in a fluidized bed reactor with reactor-scale catalyst deactivation modeling. Chem. Eng. J. 2025, 522, 167134. [Google Scholar] [CrossRef]
  172. Yousef, M.S.; González-Portillo, L.F. A novel Solar-Driven Molten-Salt methane pyrolysis system with direct Particle-to-Reactor-Wall heat Transfer: Design and Techno-Economic assessment. Energy Convers. Manag. 2027, 372, 122327. [Google Scholar] [CrossRef]
  173. Cheon, S.; Byun, M.; Lim, D.; Lee, H.; Lim, H. Parametric Study for Thermal and Catalytic Methane Pyrolysis for Hydrogen Production: Techno-Economic and Scenario Analysis. Energies 2021, 14, 6102. [Google Scholar] [CrossRef]
  174. McIvor, C.; Roy, S.; Morgan, N.; Maxwell, B.; Smallbone, A. Techno-Economic Evaluation of Scalable and Sustainable Hydrogen Production Using an Innovative Molten-Phase Reactor. Hydrogen 2025, 6, 66. [Google Scholar] [CrossRef]
  175. Razmi, A.R.; Hanifi, A.R.; Shahbakhti, M. A comparative techno-economic assessment between solar-based hydrogen production by methane pyrolysis and water electrolysis methods. Renew. Energy 2025, 242, 122504. [Google Scholar] [CrossRef]
  176. Tiam, A.; Poda, S.; Gamadi, T.; Watson, M. Uncertainty-Aware Techno-Economic and Carbon-Intensity Assessment of Permian Associated-Gas Methane Pyrolysis for Hydrogen and Solid Carbon Production. Hydrogen 2026, 7, 95. [Google Scholar] [CrossRef]
  177. Xu, Y.; Sun, P.; Elgowainy, A. Modeling and techno-economic analysis of methane pyrolysis via arc plasma for hydrogen and carbon black production. Int. J. Hydrogen Energy 2026, 221, 154181. [Google Scholar] [CrossRef]
  178. Shokrollahi, M.; Teymouri, N.; Ashrafi, O.; Navarri, P.; Khojasteh-Salkuyeh, Y. Methane pyrolysis as a potential game changer for hydrogen economy: Techno-economic assessment and GHG emissions. Int. J. Hydrogen Energy 2024, 66, 337–353. [Google Scholar] [CrossRef]
  179. Kim, S.; Lim, Y.-I.; Lee, U.-D.; Lee, Y.-J. Effect of metal loss on hydrogen production cost and greenhouse gas emissions in molten metal-based methane pyrolysis. Int. J. Hydrogen Energy 2025, 179, 151548. [Google Scholar] [CrossRef]
  180. Von Wald, G.A.; Masnadi, M.S.; Upham, D.C.; Brandt, A.R. Optimization-based technoeconomic analysis of molten-media methane pyrolysis for reducing industrial sector CO2 emissions. Sustain. Energy Fuels 2020, 4, 4598–4613. [Google Scholar] [CrossRef]
  181. Riley, J.; Atallah, C.; Siriwardane, R.; Stevens, R. Technoeconomic analysis for hydrogen and carbon Co-Production via catalytic pyrolysis of methane. Int. J. Hydrogen Energy 2021, 46, 20338–20358. [Google Scholar] [CrossRef]
  182. Lotfollahzade Moghaddam, A.; Hejazi, S.; Fattahi, M.; Kibria, M.G.; Khan, M.A. Molten metal methane pyrolysis for distributed hydrogen production: Reactor design, hydrodynamics, and technoeconomic insights. Chem. Eng. J. 2025, 524, 169812. [Google Scholar] [CrossRef]
  183. Parkinson, B.; Matthews, J.W.; McConnaughy, T.B.; Upham, D.C.; McFarland, E.W. Techno-Economic Analysis of Methane Pyrolysis in Molten Metals: Decarbonizing Natural Gas. Chem. Eng. Technol. 2017, 40, 1022–1030. [Google Scholar] [CrossRef]
  184. Parkinson, B.; Tabatabaei, M.; Upham, D.C.; Ballinger, B.; Greig, C.; Smart, S.; McFarland, E. Hydrogen production using methane: Techno-economics of decarbonizing fuels and chemicals. Int. J. Hydrogen Energy 2018, 43, 2540–2555. [Google Scholar] [CrossRef]
  185. Angikath, F.; Abdulrahman, F.; Yousry, A.; Das, R.; Saxena, S.; Behar, O.; Alhamed, H.; Altmann, T.; Dally, B.; Sarathy, S.M. Technoeconomic assessment of hydrogen production from natural gas pyrolysis in molten bubble column reactors. Int. J. Hydrogen Energy 2024, 49, 246–262. [Google Scholar] [CrossRef]
  186. Pruvost, F.; Cloete, S.; Cloete, J.H.; Dhoke, C.; Zaabout, A. Techno-Economic assessment of natural gas pyrolysis in molten salts. Energy Convers. Manag. 2022, 253, 115187. [Google Scholar] [CrossRef]
  187. Kim, D.; Oh, S.; Kim, Y.; Park, J. Sustainable hydrogen production via carbon black: Direct carbon fuel cell application for turquoise hydrogen. Chem. Eng. J. 2025, 511, 162056. [Google Scholar] [CrossRef]
  188. Keipi, T.; Tolvanen, H.; Konttinen, J. Economic analysis of hydrogen production by methane thermal decomposition: Comparison to competing technologies. Energy Convers. Manag. 2018, 159, 264–273. [Google Scholar] [CrossRef]
  189. Timmerberg, S.; Kaltschmitt, M.; Finkbeiner, M. Hydrogen and hydrogen-derived fuels through methane decomposition of natural gas – GHG emissions and costs. Energy Convers. Manag. X 2020, 7, 100043. [Google Scholar] [CrossRef]
  190. Abbaspour, A.; Pallavi, D.; Crossley, S.P.; Mba Wright, M. Techno-economic and life cycle assessment of carbon nanotube & hydrogen production integrated with a lignocellulosic ethanol biorefinery wastewater treatment. Bioresour. Technol. Rep. 2026, 36, 103089. [Google Scholar] [CrossRef]
  191. Paredes Bozzo, A.; Li, Z. Sensitivity analysis and stochastic optimization of levelized cost of hydrogen production through methane pyrolysis. Can. J. Chem. Eng. 2025, 104, 3052–3067. [Google Scholar] [CrossRef]
  192. Almansour, S.; Alkwai, L.M.; Yadav, K.; Zneid, B.A.; Pashtun, F. Predictive modeling for the mean diameter of carbon nanotubes produced by methane decomposition. Discov. Nano 2026, 21, 78. [Google Scholar] [CrossRef] [PubMed]
  193. Almansour, S.; Alkwai, L.M.; Yadav, K.; Zneid, B.A.; Pashtun, F. Data-driven models for estimating the mean diameter of carbon nanotubes in methane catalytic decomposition. Mater. Today Commun. 2026, 52, 115157. [Google Scholar] [CrossRef]
  194. Faisal, M.A.; Asif, M.A.; Al Razi, M.S.; Maheen, M.A.; Sharif, A. Reliability assessment of machine learning models for single-atom alloy catalyst screening: A chemistry-aware validation framework for methane C–H activation barrier prediction. Comput. Mater. Today 2026, 12, 100065. [Google Scholar] [CrossRef]
  195. Danilenko, M.A.; Kurmashov, P.B.; Gudyma, T.S.; Ukhina, A.V.; Shishin, A.A.; Podgornova, O.A.; Ishchenko, A.V.; Maksimovskiy, E.A.; Khajavian, M.; Liu, F.; et al. Data-driven optimization of urea-based solution combustion synthesis for Ni/Al2O3 catalysts: Unraveling the pore architecture-performance relationship in methane decomposition. Fuel 2027, 427, 140008. [Google Scholar] [CrossRef]
  196. Wang, H.; Sun, J.; Li, Y.; Deng, W. Machine learning and DFT database for C-H dissociation on single-atom alloy surfaces in methane decomposition. Sci. Data 2025, 12, 648. [Google Scholar] [CrossRef] [PubMed]
  197. Wen, Y.; Bella; Song, G.; Chang, J.; Kawi, S.; Wang, C.-H. Machine learning insights into the production and characteristics of carbon nanotubes from methane catalytic decomposition. J. Energy Chem. 2025, 104, 726–739. [Google Scholar] [CrossRef]
  198. Xue, D.; Zhang, P.; Lin, Y.; Wang, W.; Shi, J.; Hu, Q.; Lopez, G.; Moliner, C.; Sun, J.; Wang, T.; et al. Parametric study of the decomposition of methane for COx-free H2 and high valued carbon using Ni-based catalyst via machine-learning simulation. Green Energy Resour. 2025, 3, 100114. [Google Scholar] [CrossRef]
  199. Chen, Y.; Huang, X.; He, Y.; Liu, Q.; Du, J.; Yang, W.; Wang, W.; Zhang, D.; Jia, X.; Wang, H.; et al. Data-Driven Strategies for Designing Multicomponent Molten Catalysts to Accelerate the Industrialization of Methane Pyrolysis. ACS Catal. 2025, 15, 11003–11012. [Google Scholar] [CrossRef]
  200. Wen, Y.; Wang, S.; Wu, L.; Hondo, E.; Tang, C.; Jiang, J.; Ho, G.W.; Kawi, S.; Wang, C.-H. Exploring the role of process control and catalyst design in methane catalytic decomposition: A machine learning perspective. Int. J. Hydrogen Energy 2024, 72, 601–613. [Google Scholar] [CrossRef]
  201. Ehinmowo, A.B.; Nwaneri, B.I.; Olaide, J.O. Predictive modeling of hydrogen production and methane conversion from biomass-derived methane using machine learning and optimisation techniques. Next Energy 2025, 7, 100229. [Google Scholar] [CrossRef]
  202. Cheng, Z.; Huang, X.; Liu, H.; Du, J.; Ma, P.; Yin, H.; Zhang, D.; Li, H.; Chen, Y. DigMethpy: an AI-empowered digital catalysis platform for methane pyrolysis molten catalyst design. AI Agent 2026, 2, 8. [Google Scholar] [CrossRef]
  203. Shomope, I.; Al-Othman, A.; Tawalbeh, M.; Alshraideh, H.; Alraeesi, A. Enhanced hydrogen production from methane pyrolysis using CatBoost with reptile search algorithm optimization. Energy Nexus 2025, 20, 100576. [Google Scholar] [CrossRef]
  204. Pétremand, H.; Witte, J.; Kröcher, O.; Moioli, E. Machine Learning-Based Kinetic Modeling of the CO2 Methanation Reaction over an Industrial Catalyst. Ind. Eng. Chem. Res. 2025, 64, 19864–19875. [Google Scholar] [CrossRef] [PubMed]
  205. Hedman, D.; McLean, B.; Bichara, C.; Maruyama, S.; Larsson, J.A.; Ding, F. Dynamics of growing carbon nanotube interfaces probed by machine learning-enabled molecular simulations. Nat. Commun. 2024, 15, 4076. [Google Scholar] [CrossRef] [PubMed]
  206. Mendes, P.; Vermeire, F.; Van Haute, T.; Thybaut, J.W. Machine learning for catalyst design: data matters. Res. Sq. 2024, preprint. [Google Scholar] [CrossRef] [PubMed]
  207. Krasnikov, D.V.; Khabushev, E.M.; Gaev, A.; Bogdanova, A.R.; Iakovlev, V.Y.; Lantsberg, A.; Kallio, T.; Nasibulin, A.G. Machine learning methods for aerosol synthesis of single-walled carbon nanotubes. Carbon 2023, 202, 76–82. [Google Scholar] [CrossRef]
  208. Alsaffar, M.A.; Ghany, M.A.R.A.; Ali, J.M.; Ayodele, B.V.; Mustapa, S.I. Artificial Neural Network Modeling of Thermo-catalytic Methane Decomposition for Hydrogen Production. Top. Catal. 2021, 64, 456–464. [Google Scholar] [CrossRef]
  209. Rao, R.; Carpena-Núñez, J.; Nikolaev, P.; Susner, M.A.; Reyes, K.G.; Maruyama, B. Advanced machine learning decision policies for diameter control of carbon nanotubes. npj Comput. Mater. 2021, 7, 157. [Google Scholar] [CrossRef]
  210. Nikolaev, P.; Hooper, D.; Webber, F.; Rao, R.; Decker, K.; Krein, M.; Poleski, J.; Barto, R.; Maruyama, B. Autonomy in materials research: a case study in carbon nanotube growth. npj Comput. Mater. 2016, 2, 16031. [Google Scholar] [CrossRef]
  211. Bakhtyari, A.; Mofarahi, M.; Iulianelli, A. Large-scale fluidized-bed CH4 pyrolysis reactor for simultaneous COx-free H2 and carbon production: Multi-objective optimization and artificial intelligence modeling of different process schemes. Energy Convers. Manag. 2025, 336, 119885. [Google Scholar] [CrossRef]
  212. Srivastava, M.; Al-khreisat, M.J.; Patel, M.I.; Jayaprakash, B.; Mohammed, M.W.; Sahu, P.K.; Wasson, V.; Chohan, M.K.; Popal, A. Explainable machine learning modeling for predicting carbon yield in catalytic methane decomposition using multi-component catalyst systems. Mater. Today Commun. 2026, 57, 116453. [Google Scholar] [CrossRef]
  213. Cherbański, R.; Murgrabia, S.; Molga, E.; Stankiewicz, A.; Kotkowski, T. Forecasting temporal profiles of Fe/C catalyst coking in methane pyrolysis via moving window neural networks. Chem. Eng. Sci. 2027, 338, 125036. [Google Scholar] [CrossRef]
  214. Liu, H.; Cheng, Z.; Huang, X.; He, Y.; Wang, W.; Yang, W.; Li, J.; Huang, Z.; Zhao, D.; Du, J.; et al. A closed-loop framework for descriptor-empowered exploration of high-activity Co-based quaternary molten alloy catalysts for methane pyrolysis. Chem. Sci. 2026, 17, 18139–18151. [Google Scholar] [CrossRef] [PubMed]
  215. NFDI4Cat. CoreMeta4Cat: A Metadata Reference Model for Catalysis Research Data. Available online: https://nfdi4cat.github.io/CoreMeta4Cat (accessed on 14 November 2026).
  216. Burte, A.S.; Nair, A.; Grabow, L.C.; Dauenhauer, P.J.; Scott, S.L.; Abdelrahman, O.A. CatTestHub: A Benchmarking Database of Experimental Heterogeneous Catalysis for Evaluating Advanced Materials. J. Catal. 2025, 442, 115902. [Google Scholar] [CrossRef]
  217. Sudo, H.; Hasukawa, Y.; Koiwai, R.; Garcia-Escobar, F.; Nishimura, S.; Takahashi, L.; Takahashi, K. Importance of Consistent and Well-Dispersed Catalyst Datasets for Machine Learning in Oxidative Coupling of Methane. Catal. Sci. Technol. 2026, 16, 3791–3798. [Google Scholar] [CrossRef]
  218. Riley, J.; Adawi, H.; Siriwardane, R.; Poston, J.; Atallah, C. Towards a Standard Approach to the Analysis of Carbon Products Generated from Natural Gas Pyrolysis. In Proceedings of the 2024 Clearwater Clean Energy Conference; OSTI ID 2483561; Clearwater, FL, USA, National Energy Technology Laboratory (NETL), U.S. Department of Energy: Morgantown, WV, USA, 17–20 June 2024. [Google Scholar] [CrossRef]
  219. CSIRO HyResource. Hazer Commercial Demonstration Plant. CSIRO. 11 December 2024. Available online: https://research.csiro.au/hyresource/hazer-commercial-demonstration-plant (accessed on 24 October 2026).
  220. Hazer Group Ltd. Hazer partners with industry leader PSRI to accelerate large-scale commercial deployment, ASX announcement (ASX: HZR); Hazer Group Ltd: Perth, 10 June 2025; Available online: https://announcements.asx.com.au/asxpdf/20250610/pdf/06kkrfy5rgy8b0.pdf (accessed on 24 October 2026).
  221. Hazer Group Ltd. Hazer and KBR complete commercial-scale design enabling global deployment, ASX announcement (ASX: HZR); Hazer Group Ltd: Perth, 15 April 2026; Available online: https://announcements.asx.com.au/asxpdf/20260415/pdf/06yh9qnpfm9g80.pdf (accessed on 24 October 2026).
  222. Hazer Group Ltd. 2026. Appendix 4C – 30 June 2026: Quarterly Activities & Cashflow Report. ASX announcement (ASX: HZR; document 03112184). Hazer Group Ltd: Perth. Available online: https://www.aspecthuntley.com.au/asxdata/20260720/pdf/03112184.pdf (accessed on 11 November 2026).
  223. Hazer Group Ltd. Quarterly Activities Report and Appendix 4C, Quarter Ended 30 September 2026. ASX announcement (ASX: HZR); Hazer Group Ltd: Perth, 19 October 2026; Available online: https://cdn.financialreports.eu/financialreports/media/filings/65086/2026/RNS/65086_rns_2026-10-18_ee8ead48-0021-4169-8b9c-6d478eab9933.pdf (accessed on 11 November 2026).
  224. BASF; ExxonMobil. BASF and ExxonMobil Join Forces to Advance Low-Emission Hydrogen Through Methane Pyrolysis Technology, Joint News Release P233/25. BASF SE. 17 November 2025. Available online: https://www.basf.com/global/en/media/news-releases/2025/11/p-25-233 (accessed on 24 October 2026).
  225. Jenkins, S.; Fromm, C. Commercial Progress on Turquoise Hydrogen. Chemical Engineering. Available online: https://www.chemengonline.com/fullscreen/commercial-progress-on-turquoise-hydrogen/ (accessed on 24 October 2026).
  226. Swinhoe, D. Nebraska carbon black plant set to host data center. DatacenterDynamics. 13 July 2026. Available online: https://www.datacenterdynamics.com/en/news/nebraska-carbon-black-plant-set-to-host-data-center/ (accessed on 24 October 2026).
  227. Bureau, I.C.N. Graphitic Energy commissions pilot plant to produce clean hydrogen and graphite. Indian Chemical News. 13 March 2025. Available online: https://www.indianchemicalnews.com/hydrogen/lite/graphitic-energy-commissions-pilot-plant-to-produce-clean-hydrogen-and-graphite-25464 (accessed on 24 October 2026).
  228. Bailey, M. Graphitic Energy and Technip Energies enter strategic collaboration to scale up methane pyrolysis. Chemical Engineering. 27 May 2025. Available online: https://www.chemengonline.com/graphitic-energy-and-technip-energies-enter-strategic-collaboration-to-scale-up-methane-pyrolysis (accessed on 24 October 2026).
  229. Rahikka, L. Conversion of biomass into H2 and C – Hycamite business case, IEA workshop “Biomass and Hydrogen – Allies for Net Zero”; Paris, 15 May 2025, IEA Bioenergy: Paris, 2025; Available online: https://www.ieabioenergy.com/wp-content/uploads/2025/10/25_0515_Hycamite_Rahikka_Case-of-Hycamite.pdf (accessed on 24 October 2026).
  230. ChemXplore. Hycamite: Polaris confirms quality of natural gas-based battery graphite. ChemXplore. 2 September 2026. Available online: https://chemxplore.com/news/hycamite-natural-gas-battery-graphite (accessed on 24 October 2026).
  231. Business Weekly. Demand soars for Levidian graphene as Abu Dhabi project completes. Business Weekly. 16 January 2025. Available online: https://businessweekly.co.uk/posts/demand-soars-for-levidian-graphene-as-abu-dhabi-project-completes (accessed on 24 October 2026).
  232. Stiffler, L. Bill Gates-backed Modern Hydrogen lays off most of its employees after decade-long pursuit of clean energy. GeekWire. 2 December 2025. Available online: https://www.geekwire.com/2025/bill-gates-backed-modern-hydrogen-lays-off-most-of-its-employees-after-decade-long-pursuit-of-clean-energy/ (accessed on 24 October 2026).
  233. Forster, P.; Storelvmo, T.; Armour, K.; Collins, W.; Dufresne, J.-L.; Frame, D.; Lunt, D.J.; Mauritsen, T.; Palmer, M.D.; Watanabe, M.; et al. The Earth’s Energy Budget, Climate Feedbacks and Climate Sensitivity. In Climate Change 2021: The Physical Science Basis. Contribution of Working Group I to the Sixth Assessment Report of the Intergovernmental Panel on Climate Change; Masson-Delmotte, V., Zhai, P., Pirani, A., et al., Eds.; Cambridge University Press: Cambridge, UK, 2021; pp. 923–1054. [Google Scholar] [CrossRef]
  234. Al Mesfer, M.K.; Parthasarthy, V.; Danish, M.; Shah, M.; Ansari, K.B.; Ammendola, P.; Khan, M.I.; Raganati, F. A critical review on current progress and challenges in post-combustion CO2 separation from flue gas. Sep. Sci. Technol. 2024, 59, 1454–1476. [Google Scholar] [CrossRef]
  235. Al Mesfer, M.K.; Danish, M.; Ansari, K.B.; Trinh, Q.T.; Shah, M. A combined experimental and molecular modelling study on fixed bed adsorption of carbon dioxide over activated carbon. Carbon Lett. 2026, 36, 1365–1384. [Google Scholar] [CrossRef]
  236. Diab, J.; Fulcheri, L.; Hessel, V.; Rohani, V.; Frenklach, M. Why turquoise hydrogen will Be a game changer for the energy transition. Int. J. Hydrogen Energy 2022, 47, 25831–25848. [Google Scholar] [CrossRef]
  237. Zhang, Y.; Prabowo, J.; Wang, Y.; Lee, Z.; Chen, Y. When does methane pyrolysis become competitive? A life-cycle and total cost assessment of hydrogen pathways. Int. J. Hydrogen Energy 2026, 229, 154768. [Google Scholar] [CrossRef]
  238. Zhang, X.; Kätelhön, A.; Sorda, G.; Helmin, M.; Rose, M.; Bardow, A.; Madlener, R.; Palkovits, R.; Mitsos, A. CO2 mitigation costs of catalytic methane decomposition. Energy 2018, 151, 826–838. [Google Scholar] [CrossRef]
  239. Ingale, G.U.; Kwon, H.-M.; Jeong, S.; Park, D.; Kim, W.; Bang, B.; Lim, Y.-I.; Kim, S.W.; Kang, Y.-B.; Mun, J.; et al. Assessment of Greenhouse Gas Emissions from Hydrogen Production Processes: Turquoise Hydrogen vs. Steam Methane Reforming. Energies 2022, 15, 8679. [Google Scholar] [CrossRef]
  240. Postels, S.; Abánades, A.; von der Assen, N.; Rathnam, R.K.; Stückrad, S.; Bardow, A. Life cycle assessment of hydrogen production by thermal cracking of methane based on liquid-metal technology. Int. J. Hydrogen Energy 2016, 41, 23204–23212. [Google Scholar] [CrossRef]
  241. ISO 19870-1:2026; Hydrogen Technologies—Methodology for Determining the Greenhouse Gas Emissions Associated with the Hydrogen Supply Chain—Part 1: Emissions Associated with the Production of Hydrogen up to the Production Gate. International Organization for Standardization: Geneva, Switzerland, 2026. Available online: https://www.iso.org/standard/88686.html (accessed on 14 November 2026).
  242. U.S. Department of Energy. Guidelines to Determine Well-to-Gate Greenhouse Gas (GHG) Emissions of Hydrogen Production Pathways Using 45VH2-GREET, Rev. December 2025; Office of Critical Minerals and Energy Innovation: Washington, DC, USA, 2025; Available online: https://www.energy.gov/sites/default/files/2025-12/45vh2-greet-manual_december-2025.pdf (accessed on 14 November 2026).
  243. European Commission. Commission Delegated Regulation (EU) 2025/2359 of 8 July 2025 supplementing Directive (EU) 2024/1788 by specifying a methodology for assessing greenhouse gas emissions savings from low-carbon fuels. Off. J. Eur. Union 2025. Available online: https://eur-lex.europa.eu/eli/reg_del/2025/2359/oj (accessed on 12 November 2026).
  244. European Commission. Commission Delegated Regulation (EU) 2024/2620 of 30 July 2024 supplementing Directive 2003/87/EC of the European Parliament and of the Council as regards the requirements for considering that greenhouse gases have become permanently chemically bound in a product. Off. J. Eur. Union 2024, L 2024/2620. Available online: http://data.europa.eu/eli/reg_del/2024/2620/oj (accessed on 11 November 2026).
  245. European Commission. EU Sets World’s First Voluntary Standard for Permanent Carbon Removals. News. 3 February 2026. Available online: https://climate.ec.europa.eu/news-other-reads/news/eu-sets-worlds-first-voluntary-standard-permanent-carbon-removals-2026-02-03_en (accessed on 12 November 2026).
  246. Al-Ghussain, L.; Lu, Z.; Elgowainy, A.; Vyawahare, P.; Wang, M. Techno-Economic and Life-Cycle Assessment of Hydrogen Production Pathways in the Middle East and North African Region. Results Eng. 2026, 30, 110077. [Google Scholar] [CrossRef]
  247. Al Alwan, B.; Alharbi, R.M.; Ansari, K.B.; Al Mesfer, M.K.; Elkhaleefa, A.; Shah, M.; Danish, M.; Sahlabji, T. Investigating catalytic conversion of stearic acid to biofuels over Ni, Ag, Ti, and W supported date seed biochar under sub and supercritical conditions. Fuel 2026, 406, 137014. [Google Scholar] [CrossRef]
  248. Kumar, A.; Kumar, S.; Diab, M.A.; Kim, Y.; Al Alwan, B.; Shah, M. Hydrothermal in-situ generation of NiRu/NiFe nanoparticles enhancing hydrogen yields and nanometal-carbon composite formation from corn stover. Biomass Bioenergy 2026, 211, 109436. [Google Scholar] [CrossRef]
  249. Ali, A.B.M.; Ahmed, A.Y.; R, P.; Sahu, B.N.; Gomathi, T.; Kaur, G.; Matyakubov, B.; Jumanazarov, D.; Shah, M.; Diab, M.A.; et al. Synergistic trimetallic FeCoW/rGO nanocomposite as a durable and high-performance electrode for advanced supercapacitors. J. Porous Mater. 2026, 33, 171–186. [Google Scholar] [CrossRef]
  250. Ansari, K.B.; Ali, S.S.; Prajapati, A.K.; Rajnandni; Kumar, R.; Raheman, A.R.S.; Al Mesfer, M.K.; Al Alwan, B.; Shah, M.; Danish, M.; et al. MXene-polymer composite for supercapacitors and batteries: Recent progress, mechanism, challenges, costing, and future perspectives. J. Power Sources 2026, 663, 238840. [Google Scholar] [CrossRef]
  251. Shah, M.; Ansari, K.B.; Singh, S. Progress in Biomass-Plastic Copyrolysis: Thermochemical Conversion Techniques, Reaction Kinetics, Synergistic Mechanisms, and Reactor Design Innovations. Int. J. Environ. Res. 2025, 19, 256. [Google Scholar] [CrossRef]
  252. Al Mesfer, M.K.; Ansari, K.B.; Elkhaleefa, A.; Danish, M.; Shah, M.; Danish, M. Ultrasound-Assisted Pretreatment of Wastewater Treatment Plant Sludge for Enhanced Anaerobic Digestion and Biogas Production: RSM Optimization and Experimental Validation. Arab. J. Sci. Eng. 2026, 51, 22573–22589. [Google Scholar] [CrossRef]
  253. Tong, S.; Miao, B.; Zhang, L.; Chan, S.H. Decarbonizing Natural Gas: A Review of Catalytic Decomposition and Carbon Formation Mechanisms. Energies 2022, 15, 2573. [Google Scholar] [CrossRef]
  254. Karimi, S.; Bibak, F.; Meshkani, F.; Rastegarpanah, A.; Deng, J.; Liu, Y.; Dai, H. Promotional roles of second metals in catalyzing methane decomposition over the Ni-based catalysts for hydrogen production: A critical review. Int. J. Hydrogen Energy 2021, 46, 20435–20480. [Google Scholar] [CrossRef]
  255. Deng, Y.; Jeong, M.H.; Park, K.S.; Bae, J.W. Chemical-looping-based syngas production by separate CH4 decomposition and CO2 activation over mesoporous Ni-Co/MgAl2O4. Chem. Eng. J. 2025, 507, 160351. [Google Scholar] [CrossRef]
  256. Nkiawete, M.M.; Wal, R.V. Thermo-Catalytic Decomposition Comparisons: Carbon Catalyst Structure, Hydrocarbon Feed and Regeneration. Catalysts 2023, 13, 1382. [Google Scholar] [CrossRef]
  257. Neuschitzer, D.; Scheiblehner, D.; Antrekowitsch, H.; Wibner, S.; Sprung, A. Methane Pyrolysis in a Liquid Metal Bubble Column Reactor for CO2-Free Production of Hydrogen. Energies 2023, 16, 7058. [Google Scholar] [CrossRef]
  258. Parkinson, B.; Patzschke, C.F.; Nikolis, D.; Raman, S.; Hellgardt, K. Molten salt bubble columns for low-carbon hydrogen from CH4 pyrolysis: Mass transfer and carbon formation mechanisms. Chem. Eng. J. 2021, 417, 127407. [Google Scholar] [CrossRef]
  259. Yuan, X.; Sun, J.; Ma, Y.; Wang, Y.; Liu, B.; Cai, Y.; Yong, X.; Tu, X. A kinetic study of nonthermal plasma pyrolysis of methane: Insights into hydrogen and carbon material production. Chem. Eng. J. 2024, 499, 156396. [Google Scholar] [CrossRef]
  260. Perreault, P.; Boruntea, C.-R.; Yadav, H.D.; Soliño, I.P.; Kummamuru, N.B. Combined Methane Pyrolysis and Solid Carbon Gasification for Electrified CO2-Free Hydrogen and Syngas Production. Energies 2023, 16, 7316. [Google Scholar] [CrossRef]
  261. Sorcar, S.; Rosen, B.A. Methane Pyrolysis Using a Multiphase Molten Metal Reactor. ACS Catal. 2023, 13, 10161–10166. [Google Scholar] [CrossRef]
  262. Jiang, C.; Wang, I.-W.; Bai, X.; Balyan, S.; Robinson, B.; Hu, J.; Li, W.; Deibel, A.; Liu, X.; Li, F.; et al. Methane Catalytic Pyrolysis by Microwave and Thermal Heating over Carbon Nanotube-Supported Catalysts: Productivity, Kinetics, and Energy Efficiency. Ind. Eng. Chem. Res. 2022, 61, 5080–5092. [Google Scholar] [CrossRef]
  263. Hadian, M.; Buist, K.A.; Bos, A.N.R.; Kuipers, J.A.M. Single catalyst particle growth modeling in thermocatalytic decomposition of methane. Chem. Eng. J. 2021, 421, 129759. [Google Scholar] [CrossRef]
  264. Aliyev, K.; Olbricht, M. Modeling of Methane Pyrolysis in a Bubble Column Reactor Operating in Different Flow Regimes. Energies 2026, 19, 884. [Google Scholar] [CrossRef]
  265. Hadian, M.; Buist, K.; Kuipers, H. An overview of production of hydrogen and carbon nanomaterials via thermocatalytic decomposition of methane. Curr. Opin. Chem. Eng. 2023, 42, 100968. [Google Scholar] [CrossRef]
  266. Hofberger, C.M.; Dietrich, B.; Vera, I.D.; Krumholz, R.; Stoppel, L.; Uhlenbruck, N.; Wetzel, T. Natural Gas Pyrolysis in a Liquid Metal Bubble Column Reaction System—Part II: Pyrolysis Experiments and Discussion. Hydrogen 2023, 4, 357–372. [Google Scholar] [CrossRef]
  267. Tong, S.; Miao, B.; Chan, S.H. A numerical study on turquoise hydrogen production by catalytic decomposition of methane. Chem. Eng. Process. Process Intensif. 2023, 186, 109323. [Google Scholar] [CrossRef]
  268. Tong, S.; Miao, B.; Zhang, W.; Zhang, L.; Chan, S.H. Optimization of methane catalytic decomposition in a fluidized bed reactor: A computational approach. Energy Convers. Manag. 2023, 297, 117719. [Google Scholar] [CrossRef]
  269. IEA. Global Hydrogen Review 2025; International Energy Agency: Paris; Available online: https://www.iea.org/reports/global-hydrogen-review-2025 (accessed on 24 October 2026).
  270. Lumbers, B.; Agar, D.W.; Gebel, J.; Platte, F. Mathematical modelling and simulation of the thermo-catalytic decomposition of methane for economically improved hydrogen production. Int. J. Hydrogen Energy 2022, 47, 4265–4283. [Google Scholar] [CrossRef]
  271. Qian, J.X.; Chen, T.W.; Enakonda, L.R.; Liu, D.B.; Basset, J.-M.; Zhou, L. Methane decomposition to pure hydrogen and carbon nano materials: State-of-the-art and future perspectives. Int. J. Hydrogen Energy 2020, 45, 15721–15743. [Google Scholar] [CrossRef]
  272. Foley, M. Carbon Nanotube & Graphene Pricing Guide. Cheap Tubes Inc. Available online: https://www.cheaptubes.com/carbon-nanotube-graphene-pricing-guide/ (accessed on 24 October 2026).
  273. Prabowo, J.; Lai, L.; Wang, Y.; Wu, R.; Chen, Y. Sustainable carbon materials from methane pyrolysis for energy applications. Curr. Opin. Green Sustain. Chem. 2025, 52, 101004. [Google Scholar] [CrossRef]
  274. O’Brien, C. Carbon Nanotubes 2025-2035: Market, Technology & Players. IDTechEx. Available online: https://www.idtechex.com/cnt (accessed on 24 October 2026).
  275. Gamal, A.; Eid, K.; El-Naas, M.H.; Kumar, D.; Kumar, A. Catalytic Methane Decomposition to Carbon Nanostructures and COx-Free Hydrogen: A Mini-Review. Nanomaterials 2021, 11, 1226. [Google Scholar] [CrossRef] [PubMed]
  276. Hefny, M.M.; Hummel, J.; Schlemminger, P.; Quade, A.; Brandenburg, R.; Uhrlandt, D.; Weltmann, K.-D. Carbon Separation During Pure Methane Plasmalysis Using a 3D-Rotating Gliding Arc Reactor. Plasma Chem. Plasma Process. 2026, 46, 99. [Google Scholar] [CrossRef]
  277. Park, G.; Yang, S.Y.; Park, H.W.; Yun, J.S.; Saidova, N.U.K.; Lee, S.H.; Im, J.S.; Lee, K.J. Metal–support interactions program methane pyrolysis carbon into percolating MWCNT networks for high-areal-loading dry electrodes. Carbon 2026, 249, 121255. [Google Scholar] [CrossRef]
  278. Dadsetan, M.; Latham, K.G.; Khan, M.F.; Zaher, M.H.; Manzoor, S.; Bobicki, E.R.; Titirici, M.M.; Thomson, M.J. Characterization of carbon products from microwave-driven methane pyrolysis. Carbon Trends 2023, 12, 100277. [Google Scholar] [CrossRef]
  279. Kreuger, T.; Bos, A.N.R.; Kersten, S.R.A. Predicting gasification rates of pyrolytic graphite deposited from methane. Chem. Eng. J. 2022, 440, 135487. [Google Scholar] [CrossRef]
  280. Murgrabia, S.; Cherbański, R.; Molga, E.; Stankiewicz, A.; Kotkowski, T. Regeneration of bifunctional Fe/C catalyst for microwave-assisted methane pyrolysis by coke gasification with CO2. Chem. Eng. Process. Process Intensif. 2025, 216, 110421. [Google Scholar] [CrossRef]
  281. Baharudin, L.; Song, C.L.; Wong, M.K.; Chan, Y.H.; Chai, C.H.I.; Rahmat, N.; Zainol, M.M.; Samsudin, N.A.; Huurin Aman Rasidi, N.E.; Arif Nik Sofizan, N.M.; et al. Hydrogen production by methane pyrolysis in bubble column reactor using molten Co-Ru-Bi and Ni-Co-Bi catalysts: Catalytic performance and technoeconomic assessment. Chem. Eng. Res. Des. 2026, 234, 578–599. [Google Scholar] [CrossRef]
  282. Li, Y.; Yu, H.; Jiang, X.; Deng, G.; Wen, J.Z.; Tan, Z. Techno-economic analysis for hydrogen-burning power plant with onsite hydrogen production unit based on methane catalytic decomposition. Energy Convers. Manag. 2023, 277, 116674. [Google Scholar] [CrossRef]
  283. Tabat, M.E.; Omoarukhe, F.O.; Güleç, F.; Adeniyi, D.E.; Mukherjee, A.; Okoye, P.U.; Ogbaga, C.C.; Epelle, E.I.; Akande, O.; Okolie, J.A. Process design, exergy, and economic assessment of a conceptual mobile autothermal methane pyrolysis unit for onsite hydrogen production. Energy Convers. Manag. 2023, 278, 116707. [Google Scholar] [CrossRef]
  284. Chen, Z.; Zhang, R.; Xia, G.; Wu, Y.; Li, H.; Sun, Z.; Sun, Z. Vacuum promoted methane decomposition for hydrogen production with carbon separation: Parameter optimization and economic assessment. Energy 2021, 222, 119953. [Google Scholar] [CrossRef]
  285. Alkhatib, K.; Sukma, M.S.; Scott, S.A.; Zheng, Y.Y. Investigation of simultaneous production of H2 and separable carbon from CH4 in a fluidised bed of NiO/Ca2Fe2O5/CaO particles. Fuel 2024, 377. [Google Scholar] [CrossRef]
  286. Yang, L.; Liu, F.; Liu, Y.; Quan, W.; He, J. Deep regeneration of activated carbon catalyst and autothermal analysis for chemical looping methane thermo-catalytic decomposition process. Int. J. Hydrogen Energy 2018, 43, 17633–17642. [Google Scholar] [CrossRef]
  287. Ren, Z.; Zhang, J.; Bai, Y.; Wang, J.; Chen, H.; Hao, Q.; Ma, X. Unsupported nickel catalyst prepared from nickel foam for methane decomposition and recycling the carbon deposited spent catalyst. Int. J. Hydrogen Energy 2021, 46, 21853–21865. [Google Scholar] [CrossRef]
  288. Daghagheleh, O.; Schenk, J.; Zheng, H.; Zarl, M.A.; Farkas, M.; Ernst, D.; Kieush, L.; Lehner, M.; Kostoglou, N.; Obenaus-emler, R. Optimizing methane plasma pyrolysis for instant hydrogen and high-quality carbon production. Int. J. Hydrogen Energy 2024, 79, 1406–1417. [Google Scholar] [CrossRef]
  289. Rego, E.E.; Oller Nascimento, C.A.; Ribeiro, C.O. Economic analysis under uncertainty of turquoise hydrogen via methane pyrolysis. Int. J. Hydrogen Energy 2026, 225, 154378. [Google Scholar] [CrossRef]
  290. Manda, K.; Kothabai, V.; Singh, S.A.; Inkollu, S.; Boggala, S.; Chatla, A.; Vedantam, S.; Jangam, A.; Akula, V. Understanding the catalyst deactivation mechanism during methane pyrolysis for Turquoise hydrogen production over Ce–Ni-phyllosilicate. Int. J. Hydrogen Energy 2026, 253, 156280. [Google Scholar] [CrossRef]
  291. Bazri, S.; Mapelli, C.; Mapelli, L.G.; Mombelli, D.; Tommasini, M.M.S.; Lucotti, A. Thermo-catalytic methane pyrolysis for sustainable carbon production in steelmaking applications: Stainless steel catalysis and CO₂-enhanced catalyst regeneration. J. Anal. Appl. Pyrolysis 2025, 192, 107334. [Google Scholar] [CrossRef]
  292. Kludpantanapan, T.; Rattanaamonkulchai, R.; Srifa, A.; Koo-Amornpattana, W.; Chaiwat, W.; Sakdaronnarong, C.; Charinpanitkul, T.; Assabumrungrat, S.; Wongsakulphasatch, S.; Aieamsam-Aung, P.; et al. Development of CoMo-X catalysts for production of H2 and CNTs from biogas by integrative process. J. Environ. Chem. Eng. 2022, 10, 107901. [Google Scholar] [CrossRef]
  293. Inaba, M.; Kuramoto, K.; Soneda, Y. Production of Hydrogen and Solid Carbon by Methane Decomposition under Pressurized Conditions Using a Rotary Reactor and Purification of Yielded Hydrogen by Hydrogen Separation Membrane. Ind. Eng. Chem. Res. 2024, 63, 4306–4316. [Google Scholar] [CrossRef]
  294. Zeng, Y.-C.; Law, Z.X.; Tsai, D.-H. Combined Methane Cracking for H2 Production with CO2 Utilization for Catalyst Regeneration Using Dual Functional Nanostructured Particles. ACS Sustain. Chem. Eng. 2024, 12, 12200–12215. [Google Scholar] [CrossRef]
  295. Pandey, A.; Ayubkhan, F.P.; Mylipilli, N.; Thotakura, A.; Khallaghi, N. Methanol and carbon monoxide co-production via methane decomposition: techno-economic and environmental analysis. Sustain. Energy Fuels 2025, 9, 4923–4932. [Google Scholar] [CrossRef]
  296. Swartbooi, A.; Kapanji-Kakoma, K.K.; Musyoka, N.M. From Biogas to Hydrogen: A Techno-Economic Study on the Production of Turquoise Hydrogen and Solid Carbons. Sustainability 2022, 14, 11050. [Google Scholar] [CrossRef]
  297. Khan, U.M.; Sarmad, Q.; Anwar, M.; Khoja, A.H.; S.A., M.A.; Khan, Z.S.; Hassan, M.; Shakir, S. Synthesis of cobalt loaded double perovskite Sr2TiFeO6-δ (STF) as a stable catalyst for enhanced hydrogen production via methane decomposition. Int. J. Energy Res. 2021, 45, 20073–20088. [Google Scholar] [CrossRef]
  298. Allaedini, G.; Aminayi, P.; Tasirin, S.M. Methane decomposition for carbon nanotube production: Optimization of the reaction parameters using response surface methodology. Chem. Eng. Res. Des. 2016, 112, 163–174. [Google Scholar] [CrossRef]
  299. Zhang, Y.; Zhang, M.; Zhang, G.; Zhang, H. Effect of carbon deposition over carbonaceous catalysts on CH4 decomposition and CH4-CO2 reforming. Front. Chem. Eng. China 2010, 4, 481–485. [Google Scholar] [CrossRef]
  300. Otsuka, K.; Takenaka, S. Production of Hydrogen from Methane by a CO2 Emission-Suppressed Process: Methane Decomposition and Gasification of Carbon Nanofibers. Catal. Surv. Asia 2004, 8, 77–90. [Google Scholar] [CrossRef]
Figure 1. Framework of the review. Catalyst design sets how carbon grows; growth sets how carbon can be removed or the catalyst regenerated; the removal route sets the grade of the carbon product, which sets its value and, with catalyst make-up, the hydrogen cost. Blue figures indicate the number of the 95 experimental studies with harvest evidence in the dataset that report each stage; the boxes show coverage, not measured causal links.
Figure 1. Framework of the review. Catalyst design sets how carbon grows; growth sets how carbon can be removed or the catalyst regenerated; the removal route sets the grade of the carbon product, which sets its value and, with catalyst make-up, the hydrogen cost. Blue figures indicate the number of the 95 experimental studies with harvest evidence in the dataset that report each stage; the boxes show coverage, not measured causal links.
Preprints 245404 g001
Figure 2. Reporting coverage of post-reaction descriptors. Share of the 95 experimental, in-scope studies of catalytic methane decomposition with harvest evidence that report each of 14 descriptors; blue bars mark the descriptors needed to judge carbon harvest and catalyst reuse. Labels give the number of studies out of 95 and their share. Reporting frequency describes practice, not the prevalence of a mechanism.
Figure 2. Reporting coverage of post-reaction descriptors. Share of the 95 experimental, in-scope studies of catalytic methane decomposition with harvest evidence that report each of 14 descriptors; blue bars mark the descriptors needed to judge carbon harvest and catalyst reuse. Labels give the number of studies out of 95 and their share. Reporting frequency describes practice, not the prevalence of a mechanism.
Preprints 245404 g002
Figure 3. Carbon order, carbon yield, and carbon form by catalyst family. (a) Raman ID/IG of the as-produced carbon measured with 532 nm excitation and (b) carbon yield (g C per g catalyst, log scale) for families reported by at least three studies. Points are individual catalyst or condition rows, so rows from one study are correlated; blue bars are medians of all rows and open diamonds are medians of study medians, which weight each study once. Peak fitting still differs between studies, and the spread within families exceeds the differences between them; the order of families in (b) changes with the weighting. In (b), the marker gives the time on stream of the run behind each value (open, under 1 h; gray, 1–10 h; black, over 10 h; cross, not stated), and a green ring marks runs taken to deactivation; yields are the carbon formed by the end of each run. Raman ratios in (a) are likewise measured at the end of runs of different length. Rows flagged in quality control (physically implausible yields, duplicated data) are excluded, as are Raman values measured on carbon that had been purified, annealed, or regenerated (Supplementary Table S3; Dataset S4). (c) Form of the carbon as described by the authors, classed into six forms, for 188 rows from 73 experimental studies; shading gives the share of each column, numbers are rows, and column labels give rows/studies and the most common reactor with its share. Reactor and catalyst are confounded (molten media were run in bubble columns), and descriptions differ in detail, so (c) shows reported forms, not a measured distribution; row-level classes and sources are in Dataset S4. (a, b) Data from [34,35,36,37,38,39,40,41,42,43,44,45,46,47,48,49,50,51,52,53].
Figure 3. Carbon order, carbon yield, and carbon form by catalyst family. (a) Raman ID/IG of the as-produced carbon measured with 532 nm excitation and (b) carbon yield (g C per g catalyst, log scale) for families reported by at least three studies. Points are individual catalyst or condition rows, so rows from one study are correlated; blue bars are medians of all rows and open diamonds are medians of study medians, which weight each study once. Peak fitting still differs between studies, and the spread within families exceeds the differences between them; the order of families in (b) changes with the weighting. In (b), the marker gives the time on stream of the run behind each value (open, under 1 h; gray, 1–10 h; black, over 10 h; cross, not stated), and a green ring marks runs taken to deactivation; yields are the carbon formed by the end of each run. Raman ratios in (a) are likewise measured at the end of runs of different length. Rows flagged in quality control (physically implausible yields, duplicated data) are excluded, as are Raman values measured on carbon that had been purified, annealed, or regenerated (Supplementary Table S3; Dataset S4). (c) Form of the carbon as described by the authors, classed into six forms, for 188 rows from 73 experimental studies; shading gives the share of each column, numbers are rows, and column labels give rows/studies and the most common reactor with its share. Reactor and catalyst are confounded (molten media were run in bubble columns), and descriptions differ in detail, so (c) shows reported forms, not a measured distribution; row-level classes and sources are in Dataset S4. (a, b) Data from [34,35,36,37,38,39,40,41,42,43,44,45,46,47,48,49,50,51,52,53].
Preprints 245404 g003
Figure 4. Carbon and catalyst after methane decomposition, reproduced from open-access studies (CC BY 4.0; cropped and scaled, otherwise unaltered). (A) Base growth under strong metal–support interaction and tip growth under weak interaction on Ni/SBA-15 [55]. (B) Nickel particle size and encapsulation in spent Ni–Mg–Al catalysts [57]. (C) Nanotubes with nickel particles from a fluidized bed of Ni/CeZrO₂ [35]. (D) Metal encapsulated in and carried at the tips of nanotubes on Co–Fe/Al₂O₃ [58]. (E) Carbon collected above the salt layer of a Cu–Bi/NaCl reactor and (F) carbon formed with and without a NaCl cap [59]. Lower-case labels inside the panels are those of the source figures.
Figure 4. Carbon and catalyst after methane decomposition, reproduced from open-access studies (CC BY 4.0; cropped and scaled, otherwise unaltered). (A) Base growth under strong metal–support interaction and tip growth under weak interaction on Ni/SBA-15 [55]. (B) Nickel particle size and encapsulation in spent Ni–Mg–Al catalysts [57]. (C) Nanotubes with nickel particles from a fluidized bed of Ni/CeZrO₂ [35]. (D) Metal encapsulated in and carried at the tips of nanotubes on Co–Fe/Al₂O₃ [58]. (E) Carbon collected above the salt layer of a Cu–Bi/NaCl reactor and (F) carbon formed with and without a NaCl cap [59]. Lower-case labels inside the panels are those of the source figures.
Preprints 245404 g004
Figure 5. Conceptual design-for-harvest map, adapted from the failure hierarchy of Le et al. [1] and redrawn. Metal–support interaction and the form of carbon growth are proposed to decide whether carbon can be recovered as a product while the catalyst is retained; the links are hypotheses, most not yet measured together (Table 3). Counts indicate how often growth mode is reported in the dataset. It is a hypothesis map, not a validated operating diagram: the dashed border marks the region proposed as most favorable for supported catalysts, where anchoring is mostly inferred rather than measured; no single study has yet demonstrated base growth, mechanical detachment and low residual metal together, and a tip-growth route with separation after the run is described in Section 3.1 [56].
Figure 5. Conceptual design-for-harvest map, adapted from the failure hierarchy of Le et al. [1] and redrawn. Metal–support interaction and the form of carbon growth are proposed to decide whether carbon can be recovered as a product while the catalyst is retained; the links are hypotheses, most not yet measured together (Table 3). Counts indicate how often growth mode is reported in the dataset. It is a hypothesis map, not a validated operating diagram: the dashed border marks the region proposed as most favorable for supported catalysts, where anchoring is mostly inferred rather than measured; no single study has yet demonstrated base growth, mechanical detachment and low residual metal together, and a tip-growth route with separation after the run is described in Section 3.1 [56].
Preprints 245404 g005
Figure 6. Carbon purity, recovery and order by removal route. (a) Residual metal or ash in the carbon before and after the step, on the same sample (for salt-capped melts, the as-produced carbon of the same configuration), for all rows reporting both values on a wt% basis. Marker shape gives the analytical method: energy-dispersive X-ray spectroscopy (EDS) is local, X-ray fluorescence (XRF) and inductively coupled plasma (ICP) analysis are bulk, and TGA ash includes oxides and support, so values from different methods are not directly comparable. The arrow marks a value below the 50 ppm ICP detection limit [96], for which no value before washing is reported. Labels give the treatment sequence; “cap” denotes carbon formed under a molten-salt layer of the stated depth. (b) Carbon recovered or removed, grouped by basis: mass in reacting systems, volume in a reacting system, and cold-flow analogs (water/air/glass microspheres) of a molten-metal reactor, which are not reacting systems; blocks should not be ranked against each other. Becker et al. [99] is decoking of an empty, non-catalytic tube reactor; Parmar et al. [56] refers to spent catalyst containing 70 wt% carbon; Lopez-Ruiz et al. [96] is the carbon mass retained after acid washing of a 5 g sample. Wang et al. [51] is the carbon mass kept through washing of carbon skimmed from the melt. (c) Raman ID/IG of the carbon before (gray point) and after (arrowhead) the step, as measured within each study (excitation 514 or 532 nm where stated; not stated for four studies), for all 19 reported pairs; blue arrows mark more ordered carbon after the step, orange less ordered, and dark changes within ±0.02. Regeneration rows show the carbon left on the catalyst after cycling. Values from different studies differ in excitation and peak fitting and should be compared only within a study. Data from [51,56,59,83,84,96,98,99,100,101,102,103]; (c) [37,41,45,81,88,92,100,101,104,105].
Figure 6. Carbon purity, recovery and order by removal route. (a) Residual metal or ash in the carbon before and after the step, on the same sample (for salt-capped melts, the as-produced carbon of the same configuration), for all rows reporting both values on a wt% basis. Marker shape gives the analytical method: energy-dispersive X-ray spectroscopy (EDS) is local, X-ray fluorescence (XRF) and inductively coupled plasma (ICP) analysis are bulk, and TGA ash includes oxides and support, so values from different methods are not directly comparable. The arrow marks a value below the 50 ppm ICP detection limit [96], for which no value before washing is reported. Labels give the treatment sequence; “cap” denotes carbon formed under a molten-salt layer of the stated depth. (b) Carbon recovered or removed, grouped by basis: mass in reacting systems, volume in a reacting system, and cold-flow analogs (water/air/glass microspheres) of a molten-metal reactor, which are not reacting systems; blocks should not be ranked against each other. Becker et al. [99] is decoking of an empty, non-catalytic tube reactor; Parmar et al. [56] refers to spent catalyst containing 70 wt% carbon; Lopez-Ruiz et al. [96] is the carbon mass retained after acid washing of a 5 g sample. Wang et al. [51] is the carbon mass kept through washing of carbon skimmed from the melt. (c) Raman ID/IG of the carbon before (gray point) and after (arrowhead) the step, as measured within each study (excitation 514 or 532 nm where stated; not stated for four studies), for all 19 reported pairs; blue arrows mark more ordered carbon after the step, orange less ordered, and dark changes within ±0.02. Regeneration rows show the carbon left on the catalyst after cycling. Values from different studies differ in excitation and peak fitting and should be compared only within a study. Data from [51,56,59,83,84,96,98,99,100,101,102,103]; (c) [37,41,45,81,88,92,100,101,104,105].
Preprints 245404 g006
Figure 7. Activity in the last cycle relative to the first after repeated reaction–regeneration cycles, by regeneration agent. Activity is the methane conversion or rate given by each study, at the time in each cycle that the study reports. One point per catalyst and agent (the row with the most cycles). Open markers: activity rose above that of the first cycle, a measured gain reported separately from retention; one value of 607% read from a figure is omitted. Most values were read from the studies’ figures (Dataset S4). The agents were tested on different catalysts, at different temperatures and with different protocols, and the reaction time per cycle ranges from 5 min to 4 h where stated (not stated in four studies), so the carbon formed and removed per cycle differs between points; the plot describes the reported cases and does not rank the agents. Data from [35,37,40,41,44,49,52,56,58,98,127,128,132].
Figure 7. Activity in the last cycle relative to the first after repeated reaction–regeneration cycles, by regeneration agent. Activity is the methane conversion or rate given by each study, at the time in each cycle that the study reports. One point per catalyst and agent (the row with the most cycles). Open markers: activity rose above that of the first cycle, a measured gain reported separately from retention; one value of 607% read from a figure is omitted. Most values were read from the studies’ figures (Dataset S4). The agents were tested on different catalysts, at different temperatures and with different protocols, and the reaction time per cycle ranges from 5 min to 4 h where stated (not stated in four studies), so the carbon formed and removed per cycle differs between points; the plot describes the reported cases and does not rank the agents. Data from [35,37,40,41,44,49,52,56,58,98,127,128,132].
Preprints 245404 g007
Figure 8. Carbon withdrawal hardware for molten-media reactors, reproduced from open-access studies (CC BY 4.0; cropped and scaled, otherwise unaltered). (A) Liquid-tin bubble column used for reacting pyrolysis tests [149]. (B) Four concepts for withdrawing floating carbon: overflow weir, pneumatic-assisted weir, cyclone and venturi ejector, and (C) the cold-flow rig in which they were compared with water and hollow microspheres [103]; results in Figure 6b. Lower-case labels inside the panels are those of the source figures.
Figure 8. Carbon withdrawal hardware for molten-media reactors, reproduced from open-access studies (CC BY 4.0; cropped and scaled, otherwise unaltered). (A) Liquid-tin bubble column used for reacting pyrolysis tests [149]. (B) Four concepts for withdrawing floating carbon: overflow weir, pneumatic-assisted weir, cyclone and venturi ejector, and (C) the cold-flow rig in which they were compared with water and hollow microspheres [103]; results in Figure 6b. Lower-case labels inside the panels are those of the source figures.
Preprints 245404 g008
Figure 9. Longest reported operation per study by reactor platform (log scale), from the datasets and four further cited studies outside them [77,106,155,156]. Markers give how carbon left the reactor: withdrawn during the run together with catalyst (filled blue), dislodged in the reactor but collected after the run (green square; ball mill [106]), or removed after the run (open); in the empty thermal tube [138] most carbon stayed on the wall, and soot reached the filter during the run. The triangle [102] is the time at which the first carbon reached the gravity separator; the total run length is not stated. Ringed markers are elapsed campaigns whose continuity is not stated (Geißler et al. [148,157]). For the carbon-catalyst moving beds (Lee et al. [32]), the bar spans continuous runs of 24–72 h and the cross marks more than 500 h of cumulative operation over two reactors. The line on Siriwardane et al. [142] spans the 230 h test of the abstract and the 280 h with cycles of its figure, on 10% methane. In the overflow fluidized bed [145] and the moving beds carbon left with the catalyst; in the moving beds the catalyst is carbon. The dashed line marks one year (8,760 h). Data from [32,43,50,77,86,87,96,97,102,106,116,123,135,137,138,139,140,141,142,143,145,148,152,155,156,157,158].
Figure 9. Longest reported operation per study by reactor platform (log scale), from the datasets and four further cited studies outside them [77,106,155,156]. Markers give how carbon left the reactor: withdrawn during the run together with catalyst (filled blue), dislodged in the reactor but collected after the run (green square; ball mill [106]), or removed after the run (open); in the empty thermal tube [138] most carbon stayed on the wall, and soot reached the filter during the run. The triangle [102] is the time at which the first carbon reached the gravity separator; the total run length is not stated. Ringed markers are elapsed campaigns whose continuity is not stated (Geißler et al. [148,157]). For the carbon-catalyst moving beds (Lee et al. [32]), the bar spans continuous runs of 24–72 h and the cross marks more than 500 h of cumulative operation over two reactors. The line on Siriwardane et al. [142] spans the 230 h test of the abstract and the 280 h with cycles of its figure, on 10% methane. In the overflow fluidized bed [145] and the moving beds carbon left with the catalyst; in the moving beds the catalyst is carbon. The dashed line marks one year (8,760 h). Data from [32,43,50,77,86,87,96,97,102,106,116,123,135,137,138,139,140,141,142,143,145,148,152,155,156,157,158].
Preprints 245404 g009
Figure 10. Selected published estimates of the cost of hydrogen by carbon route, without (gray) and with (blue) sale of the carbon, in 2023 USD: each study’s base case or, where it gives none, the case named in Supplementary Table S4, which gives the cost metric, original value, currency year and assumptions of each case. Squares are minimum selling prices ([96,178]); circles are LCOH. Values solved for a target, secondary values cited in reviews and ranges taken from abstracts are excluded. Escalation uses the US consumer price index (CPI-U), and euro values are converted at the average exchange rate of the cost year; escalation with the Chemical Engineering Plant Cost Index (CEPCI) changes no range limit by more than $0.6 per kg. Filled blue: all carbon sold at the price each study assumed, mostly $150–1810 per t. Open blue: partial or demand-limited sale; Lumbers et al. [170] sell 10% at $10,000 per t, Tamarona et al. [171] sell 50% and are plotted at their plug-flow lower bound, and Alhamed et al. [33] use a demand-limited market model (Monte Carlo medians). Orange: carbon and steam credited (Xu et al. [177], best of four cases against the midpoint of the no-sale range). Solid lines join results for the same case that differ by the carbon credit alone; dashed lines join results that also differ in other ways. Cheon et al. [173] burn a fuel mix of 40% hydrogen and 60% methane for process heat. de Cataldo et al. [134] demonstrate a process that includes both once-through operation and central catalyst regeneration through carbon oxy-combustion with CO₂ storage. Kim, S. et al. [179] is the electrically heated Ni–Bi case at 1% metal loss. Tiam et al. [176] credit a net realized carbon value of $0.20 per kg; Yousef et al. [172] sell 58.5% of the carbon at $200 per t (open); Von Wald et al. [180] report no carbon revenue. The currency year is not stated; instead, the publication year minus one is assumed. The shaded band is unabated steam-methane-reforming hydrogen at $1–2 per kg as stated in Le et al. [1], for context only. FBR, fluidized-bed reactor; MB, moving bed; MMR, molten-metal reactor; MSR, molten-salt reactor; DCFC, direct carbon fuel cell; FB, fluidized bed; CB, carbon black; CCS, CO₂ capture and storage. Data from [33,96,134,170,171,172,173,174,175,176,177,178,179,180,181,182,183,184,185,186,187].
Figure 10. Selected published estimates of the cost of hydrogen by carbon route, without (gray) and with (blue) sale of the carbon, in 2023 USD: each study’s base case or, where it gives none, the case named in Supplementary Table S4, which gives the cost metric, original value, currency year and assumptions of each case. Squares are minimum selling prices ([96,178]); circles are LCOH. Values solved for a target, secondary values cited in reviews and ranges taken from abstracts are excluded. Escalation uses the US consumer price index (CPI-U), and euro values are converted at the average exchange rate of the cost year; escalation with the Chemical Engineering Plant Cost Index (CEPCI) changes no range limit by more than $0.6 per kg. Filled blue: all carbon sold at the price each study assumed, mostly $150–1810 per t. Open blue: partial or demand-limited sale; Lumbers et al. [170] sell 10% at $10,000 per t, Tamarona et al. [171] sell 50% and are plotted at their plug-flow lower bound, and Alhamed et al. [33] use a demand-limited market model (Monte Carlo medians). Orange: carbon and steam credited (Xu et al. [177], best of four cases against the midpoint of the no-sale range). Solid lines join results for the same case that differ by the carbon credit alone; dashed lines join results that also differ in other ways. Cheon et al. [173] burn a fuel mix of 40% hydrogen and 60% methane for process heat. de Cataldo et al. [134] demonstrate a process that includes both once-through operation and central catalyst regeneration through carbon oxy-combustion with CO₂ storage. Kim, S. et al. [179] is the electrically heated Ni–Bi case at 1% metal loss. Tiam et al. [176] credit a net realized carbon value of $0.20 per kg; Yousef et al. [172] sell 58.5% of the carbon at $200 per t (open); Von Wald et al. [180] report no carbon revenue. The currency year is not stated; instead, the publication year minus one is assumed. The shaded band is unabated steam-methane-reforming hydrogen at $1–2 per kg as stated in Le et al. [1], for context only. FBR, fluidized-bed reactor; MB, moving bed; MMR, molten-metal reactor; MSR, molten-salt reactor; DCFC, direct carbon fuel cell; FB, fluidized bed; CB, carbon black; CCS, CO₂ capture and storage. Data from [33,96,134,170,171,172,173,174,175,176,177,178,179,180,181,182,183,184,185,186,187].
Preprints 245404 g010
Figure 11. Catalyst make-up cost against carbon-to-catalyst ratio, for catalyst used once through with no recovery. The cost per kilogram of hydrogen is calculated based on the carbon-to-catalyst mass ratio of the spent solids, using the formula: cost = catalyst price × 2.98 / ratio, where 2.98 kg of carbon is formed per kilogram of hydrogen; this framework is based on Le et al. [1] and has been redrawn. The shaded band shows the total cost of SMR hydrogen, for scale. Lower panel: maximum measured carbon yield (g C per g catalyst) in each study with harvest evidence (n = 16, all supported metal catalysts); the marker indicates the state of the run at its end: run to deactivation (2), conversion falling (4), still active (1), or not reported in the text (9). The median of the study maxima is 1.8 (95% bootstrap interval 0.4–9.2); adding the 51 earlier-round studies without harvest descriptors gives 37 studies with a reported ratio and a median of 2.3. These are the carbon formed by the end of laboratory runs (median 2 h; 0.15–100 h), mostly short batch runs of varying feed dilution; as only two runs went to deactivation, they may understate the carbon these catalysts could hold, so the make-up costs read from them are illustrative estimates, not bounds for plant operation; using each study’s median instead of its maximum raises the median make-up cost at $5 per kg of catalyst from $8.3 to $14 per kg of H₂. Recovery lowers the cost only by the fraction of active catalyst returned. Data from [35,36,37,39,40,42,43,45,46,47,49,50,52,56,80,92].
Figure 11. Catalyst make-up cost against carbon-to-catalyst ratio, for catalyst used once through with no recovery. The cost per kilogram of hydrogen is calculated based on the carbon-to-catalyst mass ratio of the spent solids, using the formula: cost = catalyst price × 2.98 / ratio, where 2.98 kg of carbon is formed per kilogram of hydrogen; this framework is based on Le et al. [1] and has been redrawn. The shaded band shows the total cost of SMR hydrogen, for scale. Lower panel: maximum measured carbon yield (g C per g catalyst) in each study with harvest evidence (n = 16, all supported metal catalysts); the marker indicates the state of the run at its end: run to deactivation (2), conversion falling (4), still active (1), or not reported in the text (9). The median of the study maxima is 1.8 (95% bootstrap interval 0.4–9.2); adding the 51 earlier-round studies without harvest descriptors gives 37 studies with a reported ratio and a median of 2.3. These are the carbon formed by the end of laboratory runs (median 2 h; 0.15–100 h), mostly short batch runs of varying feed dilution; as only two runs went to deactivation, they may understate the carbon these catalysts could hold, so the make-up costs read from them are illustrative estimates, not bounds for plant operation; using each study’s median instead of its maximum raises the median make-up cost at $5 per kg of catalyst from $8.3 to $14 per kg of H₂. Recovery lowers the cost only by the fraction of active catalyst returned. Data from [35,36,37,39,40,42,43,45,46,47,49,50,52,56,80,92].
Preprints 245404 g011
Figure 12. Commercial methane-pyrolysis milestones and setbacks, January 2024 to October 2026. Events from company releases and trade press [9,219,220,221,224,226,227,231,232]; dates are those of the cited source, and all events are company-reported unless stated, and independent verification is limited. SwRI stands for Southwest Research Institute, and PSRI stands for Particulate Solid Research Inc. * Year reported; month approximate.
Figure 12. Commercial methane-pyrolysis milestones and setbacks, January 2024 to October 2026. Events from company releases and trade press [9,219,220,221,224,226,227,231,232]; dates are those of the cited source, and all events are company-reported unless stated, and independent verification is limited. SwRI stands for Southwest Research Institute, and PSRI stands for Particulate Solid Research Inc. * Year reported; month approximate.
Preprints 245404 g012
Figure 13. Reported greenhouse-gas intensity of hydrogen from methane pyrolysis in the 19 primary assessments that report it per kilogram of hydrogen as an absolute value, grouped by system boundary. Bars span each study’s pyrolysis cases (heat source, electricity grid, leakage rate, catalyst or conversion); markers give how the solid carbon was treated. Shaded bands show unabated steam methane reforming (SMR) and SMR with carbon capture and storage (CCS) as reported in the same studies. The arrow is the CO₂ that would be added if all 2.98 kg of carbon per kg H₂ were later oxidized (Equation (4)); no study includes it. Values given per MJ or MWh were converted at 141.8 MJ (higher heating value) [189] and 33.3 kWh (lower heating value) [188] per kg H₂. Two further studies report only relative values or a range shared with SMR + CCS [178,239]; studies with another functional unit are listed in Table S6. Data from [93,96,134,169,171,174,175,176,177,179,181,183,184,187,188,189,236,237,240].
Figure 13. Reported greenhouse-gas intensity of hydrogen from methane pyrolysis in the 19 primary assessments that report it per kilogram of hydrogen as an absolute value, grouped by system boundary. Bars span each study’s pyrolysis cases (heat source, electricity grid, leakage rate, catalyst or conversion); markers give how the solid carbon was treated. Shaded bands show unabated steam methane reforming (SMR) and SMR with carbon capture and storage (CCS) as reported in the same studies. The arrow is the CO₂ that would be added if all 2.98 kg of carbon per kg H₂ were later oxidized (Equation (4)); no study includes it. Values given per MJ or MWh were converted at 141.8 MJ (higher heating value) [189] and 33.3 kWh (lower heating value) [188] per kg H₂. Two further studies report only relative values or a range shared with SMR + CCS [178,239]; studies with another functional unit are listed in Table S6. Data from [93,96,134,169,171,174,175,176,177,179,181,183,184,187,188,189,236,237,240].
Preprints 245404 g013
Table 1. Closest reviews and perspectives on methane pyrolysis, and the quantitative outputs they provide, compared with this review. “Quantitative output” names what is compiled or computed across studies; “partly” means that a topic is discussed without dedicated analysis. Judgments are based on the full texts.
Table 1. Closest reviews and perspectives on methane pyrolysis, and the quantitative outputs they provide, compared with this review. “Quantitative output” names what is compiled or computed across studies; “partly” means that a topic is discussed without dedicated analysis. Judgments are based on the full texts.
Review Scope Quantitative output across studies Unit of analysis Carbon removal Carbon grade Cost ML
Sánchez-Bastardo et al. [10] thermal, catalytic and molten-media routes none (narrative) — partly partly partly no
Msheik et al. [19] catalytic and molten media, solar reactors none (narrative) — yes (molten media) partly partly no
Alves et al. [17] catalysts, reactors, regeneration none (narrative) — partly (regeneration) partly partly no
Patlolla et al. [11] technologies, heating, reactors, commercialization none (narrative) — partly partly partly no
McConnachie et al. [12] molten catalysts and slurries none (narrative) — yes partly partly no
Hantoko et al. [13] catalysts, deactivation, regeneration, economics none (narrative) — partly partly yes no
Weber et al. [28] nickel catalysts, kinetics literature data re-evaluated for particle size, stability and carbon properties; kinetic reporting guidelines catalyst partly partly no no
Alhamed et al. [14] solid, molten and plasma routes; carbon markets none (narrative) — yes (molten media) yes partly no
Zhao et al. [20] molten media none (narrative) — yes yes yes no
Prabowo et al. [26] solid carbon co-products market sizes and prices by grade carbon product yes yes partly no
Zeza et al. [16] cobalt catalysts none (narrative) — partly yes partly no
Baharudin [24] solid, plasma and molten systems none (narrative) — partly partly partly no
Yu et al. [23] molten metals and salts, bubble columns none (narrative; values quoted in the text) — yes (skimming and buoyant separation) partly partly (quoted TEA values) no
Moghaddam et al. [25] mechanisms to markets and industry cost and energy figures as reported technology partly yes yes no
Le et al. [1] supported catalysts for pyrolysis make-up cost equation, failure hierarchy and price guardrails; no compiled data concept yes (as design requirement) partly yes no
Musa et al. [8] harmonized techno-economics and life cycle of pyrolysis against reforming, for hydrogen, syngas and methanol parametric cost and climate decision space under harmonized boundaries process scenario partly partly yes no
Portillo et al. [15] supported Ni, Co and Fe catalysts carbon yields for more than 300 catalysts (yield only) catalyst partly partly partly no
Ba-Tuq et al. [29] catalysts, kinetics, reactor design catalyst, reactor and TEA indicators tabulated as reported study partly partly yes no
Zhang et al. [27] carbon black from pyrolysis properties, applications and market constraints carbon product partly yes partly no
Aman Rasidi et al. [21] molten media in bubble columns none (narrative) — yes partly partly no
This review removal route, carbon grade, catalyst make-up and cost co-reporting of recovery, contamination and catalyst fate; medians with study-weighted checks; measured carbon-to-catalyst ratios on the make-up framework; escalated costs; ML validation audit condition row, study and cost case yes, by route and event yes yes, with carbon-price term yes (validation audit)
Table 2. Carbon removal and regeneration routes compared by event: whether carbon is detached, withdrawn from the reactor, purified or gasified, and where the carbon and the active phase go. Ranges are those reported in the studies cited in each row; “not reported” means the datasets lack a study that provides the value.
Table 2. Carbon removal and regeneration routes compared by event: whether carbon is detached, withdrawn from the reactor, purified or gasified, and where the carbon and the active phase go. Ranges are those reported in the studies cited in each row; “not reported” means the datasets lack a study that provides the value.
Route (studies) Event Carbon goes to Active phase goes to Carbon recovered Purity or residual metal reached Main limitation
Sieving, ultrasound, magnetic separation [35,56,98] detachment after the run solid product retained; recalcined and reused in one study 10–50% <0.5 wt% metal when it works; ~35 wt% catalyst when it does not recovery low unless catalyst designed to shed carbon
In situ shear or abrasion [44,97,106] detachment during the run solid, collected after the run retained; 5–15% mass lost per cycle in one study 86% carbon closure (one study) <0.1 wt% residue (one study) laboratory scale only
Acid leaching [96,100] purification after withdrawal solid product dissolved; resynthesized from the leachate in one study 90.8–94.9% (one 5 g lab study) <50 ppm metal (ICP detection limit); ~7 wt% encapsulated residue with ore encapsulated metal persists; reagent and waste
Molten metal, collection [59,83,84,116] withdrawal by flotation solid at melt surface melt retained; loss with carbon 86–96% collected after the run (tin column) 52–83 wt% metal unwashed (Bi-based melts, EDS) melt carry-over and loss
Molten metal with salt cap [59,83] withdrawal plus washing solid product melt retained; salt to be recovered not reported 2.2–5 wt% metal; up to 98 wt% C after wash and heat salt trapped in carbon
Thermal (≥1500 °C) or electrochemical [88,101] purification of collected carbon solid product not applicable not reported 99.6–99.8 wt% C energy per tonne not reported
O₂ or air [41,58] regeneration CO, CO₂ reused; sintering or restructuring possible 0% (gasified) not applicable product lost; CO₂ formed
CO₂ [40,49] regeneration CO reused 0% (gasified) not applicable product lost; CO formed
Steam [35,98] regeneration, partial CO, H₂; ~12% left as nanotubes reused ~10% sieved before gasification (one study) not applicable incomplete gasification
H₂ pulses [43] regeneration CH₄ reused 0% not applicable consumes 6–23% of the H₂ produced
Central oxy-combustion with CO₂ storage, modeled [134] regeneration off site CO₂ to storage 95% returned (assumed) 0% not applicable transport, oxygen and electricity cost
Table 3. Chains of evidence from catalyst to cost: links measured in the same study (M), modeled or assumed (Mod), or not reported (—). Values are as reported.
Table 3. Chains of evidence from catalyst to cost: links measured in the same study (M), modeled or assumed (Mod), or not reported (—). Values are as reported.
Study and system Growth mode Carbon-to-catalyst ratio Metal in carbon as produced Removal and carbon recovered Metal in carbon after removal Catalyst fate Application or value test Cost input
Ni–Cu–Zn/Al₂O₃, fluidized bed [56] M (tip) M (0.4–2.0) — M: ultrasound and magnet, 45–50% M: <0.5% M: recalcined, >90% conversion over 5 regenerations — —
Ni–Cu, Ni–Pd [96] — M — M: HNO₃ wash, 90.8–94.9% M: <50 ppm M: metal dissolved and resynthesized; carbon reused as support characterized against commercial nanotubes; no application test Mod: TEA built on the measured metrics
Fe/CaO, fluidized bed [98] M (base) — — M: sieving recovered about 10% of the carbon M: 0.02–1.47 wt% catalyst (catalyst mass, not elemental metal) in the sieved carbon over 8 cycles M: steam-regenerated over 8 cycles — —
Ni–Bi with bromide cap [83] not applicable not applicable M: ~83 wt% (no cap, EDS) — M: <5 wt% with cap; configuration-specific melt retained — —
molten tin, solar column [84] not applicable not applicable M: 3.6–7.6 wt% Sn (EDS) M: 86–96% collected after the run — melt retained — —
Fe on corncob char [46] M (tip) M (1.2) M: 19.8 wt% Fe (EDS) none; carbon and catalyst used together not applicable used with the carbon M: CO₂ gasification reactivity against coke —
Ni–Fe, Ni–Co/SiO₂ [36] M (tip, mixed) M (2.3–2.5) M: ~25–30 wt% (TGA) — — — — —
carbon catalyst, moving bed [32] not applicable not applicable (carbon catalyst) not applicable M: screw discharge at 400 g h⁻¹; 30–35% entrained to cyclone and filter not applicable carbon is the bed inventory — — (energy 9.7–11 kWh per kg H₂)
Fe, moving bed (model) [134] — Mod (5) — none; carbon burned not applicable Mod: 95% returned — Mod
Table 4. Longest reported runs by reactor platform, one study per row, from both datasets and two of the four further studies used in Figure 9 [106,155]; the other two [77,156] do not add a platform row. Run lengths and conditions are as reported; n.s., not stated.
Table 4. Longest reported runs by reactor platform, one study per row, from both datasets and two of the four further studies used in Figure 9 [106,155]; the other two [77,156] do not add a platform row. Run lengths and conditions are as reported; n.s., not stated.
Platform and study Run length (h) Duration type Scale and feed Carbon during the run Recovery or carry-over reported Main issue reported
Moving bed, carbon catalyst [32] >500 in total; runs of 24–72 cumulative; continuous runs 10 and 15 cm tubes; pure CH₄, 1000–1080 °C screw discharge at 400 g h⁻¹; 30–35% entrained to cyclone and filter carbon is the catalyst wall deposition; conversion 20–37%
Molten tin column [148] 360 elapsed (15 days), continuity n.s. packed quartz rings; n.s. none; accumulated in the head space 0.70 wt% Sn in carbon no withdrawal installed
Molten Ni–Bi column [116] 170 run 1065 °C; n.s. none; floated to the surface n.s. n.s.
Molten tin column with discharge [102] >5.7 (total n.s.) time to first carbon at separator scaled column; n.s. pneumatic; flotation–gravity ~30 vol% before outlet blocked (pneumatic) outlet blockage, melt weeping
Molten salt column [87] 50 run n.s. none n.s. n.s.
Molten salt electrolyzer [152] 100 run at constant current LiCl–NaCl–KCl melt, 15 cm; 550 °C; 1 A none n.s. about 30% conversion; traces of Cl₂ in the exit gas
Fluidized bed, Fe–Al₂O₃ [142] 230–280 test with cycles 500 g catalyst, 6 cm bed; 10% CH₄ fines with catalyst elutriated to filters n.s. >80% conversion for 160–165 h only
Fluidized bed, Ni–Mn/Al₂O₃ [145] 5–7 runs pressurized; ~5 kg C/day overflow of carbon with catalyst catalyst not separated catalyst leaves with the product
Ball mill, Re/Ni [106] 240 run milling balls; 450 °C knocked off in situ, collected after the run n.s. 7.75% conversion
Fixed bed, Ni–Fe [155] 210 run 100 mg; 28.6% CH₄ none not applicable conversion fell to about 40%
Packed bed, wood charcoal [135] 35 run n.s. none not applicable plugging on cooling
Membrane reactor, Ni/SiO₂–Al₂O₃ [43] 100 25 cycles with H₂ regeneration n.s. partly hydrogenated between cycles n.s. H₂ consumed for regeneration
Coated tube [137] 46.4 run n.s. none n.s. metal at filament tips
Thermal tube, no catalyst [139] 8 run steel tube, 950 °C none n.s. aromatic condensate blocked the exit line
Table 5. Proposed reporting checklist for carbon harvest and catalyst reuse in methane pyrolysis, with the share of the 95 experimental studies in the dataset that now report each item. Each tier applies only to studies that include that step; for Tier 5 the share refers to the 26 primary emissions assessments in Table S6.
Table 5. Proposed reporting checklist for carbon harvest and catalyst reuse in methane pyrolysis, with the share of the 95 experimental studies in the dataset that now report each item. Each tier applies only to studies that include that step; for Tier 5 the share refers to the 26 primary emissions assessments in Table S6.
Tier Applies to Report Share of studies reporting now
1. Carbon formed every experimental study carbon yield per g catalyst and per g metal, with the basis (fresh catalyst, metal, whole bed with diluent, or spent solids); feed composition and dilution; time on stream with the conversion at the start and end, stating whether the run reached deactivation, and the average rate (g C per g catalyst per hour); growth mode with the transmission electron microscopy (TEM) evidence; residual metal in the as-produced carbon with method, sample basis and detection limit (bulk ICP or XRF preferred to local EDS; for TGA ash, state whether the support is included); Raman ID/IG with laser wavelength and fitting yield 30/95; growth mode 16/95; residual metal 36/95; Raman 56/95
2. Removal studies that recover solid carbon route, sequence and conditions; carbon withdrawn and carbon collected, each as a fraction of carbon formed; carbon and metal mass closure with its uncertainty; residual metal, salt and purity after removal, by a bulk method with detection limit; Raman and surface area before and after; catalyst recovered and reused, as fractions; reagent and energy use per kg of carbon; any test against a reference product removal step 56/95; purity 31/95; fraction recovered in 5 of 56 removal studies
3. Regeneration studies that gasify carbon agent, temperature and time; fraction of carbon gasified and its products; activity metric and the time in each cycle at which it is measured; first- and last-cycle absolute values as well as their ratio, distinguishing a gain (above 100%) from retention; metal lost per cycle; structure of any residual carbon regeneration 35/95; cycles 30/95; Raman after regeneration in 5 of 35
4. Process and cost reactor and techno-economic studies run length, stating whether a single uninterrupted run, a campaign or a cumulative total; carbon withdrawn versus produced; metal or salt carried over; catalyst or melt make-up per kg H₂; cost metric (LCOH or minimum selling price), with and without carbon sale; carbon price, grade, fraction sold and fraction treated; purification cost per tonne treated; hydrogen purity and pressure; currency year fraction recovered in 6 of 71 experimental reactor rows; purification cost per tonne in one study (a nanotube grade)
5. Emissions studies that report greenhouse-gas emissions functional unit of 1 kg H₂ at stated purity and pressure; boundary (direct, with purchased energy, or cradle-to-gate with gas supply); heat source and electricity intensity; methane supply emissions and leakage rate with GWP100 and GWP20; the carbon treated three ways (no credit, allocation with its method and share, system expansion naming the displaced product); carbon end use and the fraction later oxidized over a stated horizon; emissions of purification residues and of catalyst or melt make-up of 26 primary assessments (Table S6): leakage rate stated or varied in 4; carbon allocated or credited in 4; carbon fate stated in 10; oxidized fraction quantified in none
Table 6. Status of selected methane-pyrolysis developers, from company filings, releases and trade press (accessed 24 October 2026; Hazer and Monolith checked against their own records on 11 November 2026). Operation, announcements and market tests are listed separately.
Table 6. Status of selected methane-pyrolysis developers, from company filings, releases and trade press (accessed 24 October 2026; Hazer and Monolith checked against their own records on 11 November 2026). Operation, announcements and market tests are listed separately.
Developer Route Carbon handling Operated (reported) Designed or announced Customer tests or sales Basis Sources
Hazer fluidized bed, iron-ore catalyst graphite leaves with the bed solids; cyclone and filtration 100 t H₂ a⁻¹ (nameplate) demonstration plant, in campaigns 30 kt H₂ a⁻¹ design package with KBR (April 2026); utility pre-feasibility study asphalt tests with Boral; graphite purified to >99.99% for battery tests; no sales reported (September 2026) ASX filings [219,220,221,222,223]
BASF and ExxonMobil moving bed, electric heating not disclosed test plant at Ludwigshafen Baytown demonstration, up to 2,000 t H₂ and 6,000 t C a⁻¹ not disclosed company [224,225]
Monolith plasma gas-phase carbon black commercial plant; feed switched from natural gas to carbon black oil in 2025 expansion with four reactors; campus plan includes a data center carbon black sold commercially operator record; trade press [9,226]
Graphitic Energy (formerly C-Zero) molten media (as C-Zero) not disclosed pilot at Southwest Research Institute, up to 1 t C a day scale-up collaboration with Technip Energies not disclosed trade press [225,227,228]
Hycamite thermocatalytic not disclosed pilot unit at Kokkola design for 2 kt H₂ a⁻¹ anode material at 99.95% C and 361 mAh g⁻¹ (company-reported) company [229,230]
Levidian microwave plasma graphene unit at an Abu Dhabi National Oil Company (ADNOC) site with Baker Hughes (2025) — not disclosed trade press [231]
Modern Hydrogen methane pyrolysis devices — most staff laid off, late 2025 — — trade press [232]
Table 7. Minimum rules for greenhouse-gas accounting of hydrogen from methane pyrolysis, with the evidence from the 26 primary assessments (Table S6) that motivates each.
Table 7. Minimum rules for greenhouse-gas accounting of hydrogen from methane pyrolysis, with the evidence from the 26 primary assessments (Table S6) that motivates each.
Item Rule Evidence from the assessments
Functional unit 1 kg H₂ at stated purity and pressure; report other products per kg H₂ as well 5 of 26 use another unit
Boundary cradle-to-gate as default; report direct, purchased-energy and supply-chain terms separately 8 of 26 count direct emissions only
Methane supply leakage rate and supply-chain emissions as variables; results with GWP100 and GWP20 (fossil CH₄ 29.8 and 82.5 [233]) 4 of 26 state or vary a leakage rate; each 1% adds ≥1.2 kg CO₂-eq per kg H₂ (Equation (4))
Heat and electricity heat source, share of methane or hydrogen burned, purge treatment, electricity intensity direct emissions from 0 to 24.6 kg CO₂ per kg H₂ within one flowsheet family [174]
Carbon treatment three results: no credit; allocation with method and share; system expansion naming the displaced product and its own life cycle the choice moves one harmonized result between 5.1 and 12.6 [237]
Carbon fate end use, evidence of permanence and the oxidized fraction fox over a stated horizon; never count the same carbon as stored and as displacing a product that would itself be oxidized fox = 1 adds 10.9 kg CO₂ per kg H₂; no study quantifies fox
Treatment and make-up energy, acid and salt of purification; embodied emissions of catalyst or melt make-up 1% Ni–Bi loss adds 1.75 kg CO₂-eq per kg H₂ [179]
Conversion and recycle methane conversion, recycle ratio and fate of unconverted gas with a carbon-black credit, the advantage over reforming is lost below about 50–55% conversion [237]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.
Copyright: This open access article is published under a Creative Commons CC BY 4.0 license, which permit the free download, distribution, and reuse, provided that the author and preprint are cited in any reuse.