Preprint
Article

This version is not peer-reviewed.

Roasting Temperature and Particle Size Govern Gold Release and Desulfurization of a Historical Peruvian Pyritic Tailing

Submitted:

12 November 2026

Posted:

13 November 2026

You are already at the latest version

Abstract
Tailings containing pyrite generate acid drainage and still contain gold that direct cyanidation fails to recover. The Santa Catalina tailings (Peru), containing 2.4 g/t Au, 62 g/t Ag, and about 60% pyrite, were studied. Although more than 99% of the pyrite was liberated, direct cyanidation extracted only 13–14% of the gold. The tailings were roasted at temperatures between 400 and 800 °C using two particle sizes, and the calcines were cyanidated. Scanning electron microscopy revealed 2 µm gold particles and silver tellurides containing gold in the pyrite of the calcines at 400–500 °C. The pyrite transformed into porous hematite from the edge toward the center, passing through pyrrhotite. Grinding to 95% −38 µm lowered the temperature required for sulfur removal by about 100 °C compared to 60% −75 µm. The optimal condition—600 °C with fine grinding—extracted 52.7% of the gold and 37.7% of the silver. At 800 °C, gold extraction dropped to 25–27%, likely due to the formation of Zn and Cu ferrites. Temperature accounted for 68% of the variation in gold extraction. To scale up the process, it is advisable to first concentrate the pyrite by flotation and to reduce the high cyanide consumption caused by copper.
Keywords: 
;  ;  ;  ;  ;  ;  

1. Introduction

Mining produces enormous volumes of tailings, and many old deposits were left without proper closure, at risk of failure and pollution [1]. In Peru, the official inventory lists 6903 mining environmental liabilities [2]. For decades these tailings were seen only as a problem. Today they are also beginning to be seen as a resource: they contain metals that the processes of their time could not recover, and reprocessing them can pay for part of their remediation [3,4,5]. There are already examples with copper and pyrite in tailings from Serbia and Chile [6,7].
The risk posed by these deposits comes mainly from pyrite. When it oxidizes in contact with air and rainwater, it produces sulfuric acid and releases metals into the environment, a process that can remain active for decades after mine closure [8,9,10]. The Santa Catalina tailings dam in Shorey (Quiruvilca, La Libertad) is a clear case. It holds pyrite-rich tailings from polymetallic flotation at the head of the Moche River basin, whose water is used for agriculture in the valley. High concentrations of Fe, Zn, Pb and As have been measured in this river since the 1980s [11], and in 2020 the upper basin recorded a pH of 2.6, with 82 mg/L Fe, 27 mg/L Zn and 2.1 mg/L As [12].
The same tailing contains 2.4 g/t gold and 62 g/t silver. The problem is that this gold does not dissolve easily. In pyritic ores, much of the gold is locked inside pyrite, as grains a few micrometers across or even invisible under the microscope, and cyanide cannot reach it [13,14,15]. In gold deposits of southern Peru, gold occurs precisely as micrometric grains within pyrite, together with tellurides [16]. Gold and silver tellurides are another source of refractoriness and usually require an oxidative pretreatment such as roasting [17,18]. When that pretreatment fails to destroy the pyrite, the trapped gold barely responds even to very fine grinding [19].
To release this gold, the pyrite must be broken down. The industrial options are pressure oxidation, bio-oxidation and roasting [20]. Oxidative roasting is the simplest: between 500 and 700 °C, pyrite reacts with oxygen in the air, passes through pyrrhotite and ends up as porous hematite [21,22,23]. The gold then sits inside an oxide skeleton whose pores cyanide can penetrate. Temperature, however, has an optimum. In pyrite concentrates, gold extraction rises up to 500–600 °C and then falls, because the oxide sinters, its pores close and the gold becomes locked again [13,24]. This optimum coincides with the maximum pore volume of the calcine [14,25,26], and the roasting atmosphere also changes how the gold responds to cyanidation [27].
Almost everything known comes from pyrite-rich, high-grade concentrates. A tailing is different: the pyrite is diluted in quartz and clays, part of it has already oxidized to sulfates, and it is usually accompanied by copper minerals that consume cyanide [28,29]. In addition, the particle size of the calcine influences where the undissolved gold remains trapped [30]. Even so, few studies have evaluated roasting temperature and particle size together in historical pyritic tailings, or linked what happens inside the particle with what is finally extracted.
In this work, we roasted the Santa Catalina tailing at five temperatures (400–800 °C) and two particle sizes (60% −75 µm and 95% −38 µm), and then cyanided the calcines. We followed the transformation of pyrite with X-ray diffraction (XRD) and scanning electron microscopy (SEM), located the gold before and after roasting, and used statistics to measure the weight of each variable. We aim to answer a practical question: under what conditions is it worth roasting a pyritic tailing to recover its gold while removing its capacity to generate acid drainage?

2. Materials and Methods

2.1. Sampling and Preparation

About 100 kg of tailing was collected from the Santa Catalina tailings dam (Shorey, Quiruvilca, La Libertad; UTM 17S, 795,937 E, 9,112,096 N), and a 20 kg composite split was used for the experiments. The sample was dried at 80 °C for 24 h in a Schemin oven, homogenized and split into 1 kg lots with a rotary splitter. The particle size distribution was determined by sieving from 20 mesh (850 µm) to 400 mesh (38 µm) with ELE International sieves (ASTM E11) on a Tyler RX-29-16 Ro-Tap shaker. The grinding curve was built with 1 kg lots in an 8 × 10 in stainless-steel ball mill (Edjar) with 11 kg of balls, at 66.7% solids, for 5, 10, 15 and 20 min, and the product of each time was sieved together with the unground feed. A grinding time of 7 min was selected for 60% −75 µm (#200 mesh), read from the curve of material passing #200 mesh. For 95% −38 µm (#400 mesh), the linear regression of material passing #400 mesh over 0–20 min (y = 2.020x + 11.434; R² = 0.996) predicted the target at about 41 min, but the verification grinds fell below that trend (82.9% −38 µm at 37.3 min and 90.3% at 45 min), because grinding loses efficiency as the product becomes finer. A value of 95.2% −38 µm was reached at 55 min, and this time was used for all fine grinds (Figure S1). Hereafter, these sizes are referred to as #200 mesh and #400 mesh. The experimental flowsheet is shown in Figure 1. Part of the roasting and cyanidation tests was presented in the undergraduate thesis of two of the authors [31]; the iron phase balance, the statistical analysis, the roasting kinetics, the metal retention analysis and the mineralogical interpretation are new to this work.

2.2. Characterization

Solid samples (heads, calcines and residues) were analyzed at the Chemistry Laboratory of the Geological, Mining and Metallurgical Institute of Peru (INGEMMET), accredited under ISO/IEC 17025 by INACAL (registration LE-182). Gold was determined by fire assay with atomic absorption finish, and Ag, Cu, Pb, Zn and Fe by atomic absorption spectrometry (AAS; Thermo Scientific iCE 3300) after four-acid digestion (HCl, HNO₃, HF and HClO₄). In the unroasted tailing, minor and trace elements, including As and Sb, were determined after four-acid digestion by inductively coupled plasma optical emission spectrometry (ICP-OES; Varian 735-ES) and mass spectrometry (ICP-MS; PerkinElmer NexION 300D). Total sulfur was determined by gravimetry as barium sulfate, and loss on ignition at 950–1000 °C. Arsenic in the 600 °C calcines was determined by AAS after acid digestion on the PerkinElmer AAnalyst 400 spectrometer (Section 2.4). XRD patterns were recorded on a Shimadzu XRD-7000 diffractometer with Cu Kα radiation (40 kV, 30 mA) from 3° to 70° 2θ, with a step of 0.02° and a scan speed of 2°/min. Phases were identified with the ICDD PDF-4+ 2023 database and semi-quantified by the reference intensity ratio (RIR) method. The tailing and the ten calcines were examined with a Carl Zeiss EVO MA 15 SEM using a backscattered electron detector and an energy-dispersive X-ray spectrometer (EDS) (20 kV, high vacuum) at the INGEMMET Petromineralogy Laboratory (Technical Report No. 007-2024-INGEMMET/DL-LP). The spot compositions cited (As in pyrite; Zn and Cu in the oxides) are semi-quantitative, obtained by EDS and taken from that report, which does not include the spectra. The degree of liberation and the mineralogical composition were determined by counting free and locked particles and classifying their intergrowth types. Weighings were made on RADWAG precision (0.01 g) and analytical (AS 200 R2 PLUS, 0.0001 g) balances. Analytical quality was controlled with blanks, duplicates and certified reference materials (Test Report No. 022-2024-INGEMMET/DL-LQ): all blanks were below the method detection limits, duplicates agreed within 2.6% relative standard deviation (0.1–1.2% for Au and below 0.6% for S), and the recoveries of the certified reference materials were 98–102% for Au, 97–100% for S and 86–115% for Ag, Cu, Pb, Zn and Fe.
Because semi-quantitative XRD does not close the mass balance in pyrite-rich samples, the distribution of Fe among phases was calculated with a chemistry-constrained balance. First, the sulfur bound to base-metal sulfides (0.78% in the tailing, estimated from Zn, Pb and Cu and corrected for mass loss) was subtracted. The remaining sulfur was assigned to pyrite and, when XRD detected sulfates, split between pyrite and iron sulfate according to their XRD proportions. The associated Fe was calculated stoichiometrically, and the remaining Fe was distributed between magnetite/maghemite and hematite according to their XRD proportions. The balance closed within 1.3% of total Fe.

2.3. Roasting

Samples of 100 g were roasted in refractory porcelain dishes inside an electric muffle furnace (Schemin MD 20L) with a thermocouple, a pyrometer (±5 °C) and a fume extraction hood, in air, at 400, 500, 600, 700 and 800 °C for each particle size. Each test lasted 3 h, with the bed stirred every 15 min. Five 100 g batches were roasted for each condition to obtain enough calcine for characterization and cyanidation. Mass loss was followed in two of these batches; because the two records agreed closely, the remaining batches were used only to accumulate calcine, and the calcines of each condition were combined for analysis. Mass loss (ML) was recorded at 15, 30, 60, 90 and 150 min, and at 600 °C the chemical composition was analyzed at each time. The calcines were cooled in air and characterized by XRD, chemical analysis and SEM. Desulfurization was calculated with a correction for mass loss:
DS (%) = [1 − Sc (1 − ML/100)/S0] × 100
where S₀ and Sc are the sulfur grades of the tailing and the calcine (%) and ML is the mass loss (%). The retention of Au and Ag in the calcine was calculated in the same way, using the metal grades instead of sulfur. For the kinetics, conversion was defined as α = ML(t)/MLmax, where MLmax is the mass loss at 800 °C and 150 min for each particle size. Rate constants were obtained by fitting g(α) = 1 − (1 − α)1/3 (shrinking core, chemical control) and g(α) = 1 − 2α/3 − (1 − α)2/3 (product-layer diffusion) to the 0–30 min data, and the apparent activation energy was calculated with the Arrhenius equation between 400 and 800 °C.

2.4. Cyanidation

Bottle-roll cyanidation was performed with 50 g of calcine or unroasted tailing and 200 mL of solution (20% solids), 3000 ppm NaCN and pH 11 adjusted with NaOH, with agitation for 72 h. An independent bottle was used for each time (12, 24, 48 and 72 h), so each point of the leaching curve comes from a pulp not disturbed by earlier sampling. Because the bottles are independent, time could be included as a factor in the ANOVA (Section 2.5). At 10 h, free cyanide (titration with AgNO₃ on a 10 mL aliquot) and pH were measured and NaCN was replenished to 3000 ppm in all bottles. At 12 h the first bottle was stopped and its pregnant solution was sampled for Au and Ag. The remaining bottles were stopped at 24, 48 and 72 h; in each one, free cyanide, Au and Ag were determined, and NaCN in the bottles still running was replenished to 3000 ppm. Au and Ag in the pregnant solutions were analyzed by AAS on a PerkinElmer AAnalyst 400 spectrometer, with calibration curves prepared in cyanide medium. In the residue of the 72 h bottle, Au was determined by fire assay and Ag by AAS after acid digestion. The calculated extraction was obtained from the calculated head (metal in solution plus metal in residue), and the assayed extraction as (head grade − residue grade)/head grade. A difference below 5 percentage points between the two was used as the quality criterion.

2.5. Statistical Analysis

Roasting results (mass loss, residual sulfur and desulfurization) are reported descriptively, because sulfur was assayed once on the combined calcine of each condition. Au and Ag extraction was analyzed as an unreplicated 2 × 5 × 4 factorial (n = 40 bottles), with the main effects and two-way interactions, using the three-way interaction as the error term (12 degrees of freedom). Type II sums of squares, α = 0.05 and one-tailed F tests were used, with statsmodels 0.15.0 in Python 3.13. The percentage contribution of each source was calculated as its sum of squares divided by the total sum of squares.

2.6. Use of Generative Artificial Intelligence Tools

During the preparation of this work, the authors used Claude Opus 5.5 (Anthropic, San Francisco, CA, USA), a generative artificial intelligence model, to support: (i) writing the Python code (statsmodels and matplotlib) for the ANOVA, the kinetic fits and the figures; (ii) the literature search, whose references were verified by the authors against the original sources; and (iii) drafting, language editing and translation of the text into English. In all cases, the work started from the authors’ experimental data, analyses and interpretations. All graphs and the mechanism schematic were produced with Python code (matplotlib) from the authors’ experimental data; no AI image-generation tools were used. The SEM images are originals from INGEMMET and were only cropped and arranged into panels. The authors designed the study, performed all experiments, interpreted the results, and reviewed, verified and edited all content.

3. Results

3.1. Tailing Mineralogy and Gold Deportment

The tailing is pyritic and medium-grained: only 26.7% passes 75 µm. Its chemical composition (Table 1) corresponds to about 60% normative pyrite, consistent with the total Fe. XRD also identified quartz, pyrophyllite, muscovite, kaolinite and melanterite (4.7–7.5%), a sulfate that indicates pyrite oxidation in the dam.
SEM showed pyrite liberation of 99.2% (#200 mesh) and 100% (#400 mesh), with sphalerite, pyrrhotite, tennantite, galena, arsenopyrite, chalcopyrite and enargite as minor phases. The tailing contains 0.50–0.53% As and 0.04–0.05% Sb. No free gold was observed in the unroasted tailing. Gold was found in the still-unoxidized pyrite of the #200 mesh calcines at 400 and 500 °C, as native gold inclusions of about 2 µm and as Ag tellurides (probably hessite) with Au, also about 2 µm in size (Section 3.3); in that pyrite, about 10% of the particles contain around 1% As. That these inclusions were not observed in the unroasted tailing is attributed to their scarcity and size, which make them unlikely to appear in a polished section in which 426 to 958 particles were counted. Because the pyrite at 400–500 °C and #200 mesh remains nearly intact, these inclusions represent gold already present in the tailing. Direct cyanidation extracted 12.8% of the Au at #200 mesh and 14.2% at #400 mesh.

3.2. Sulfur Removal and Phase Evolution

Fine grinding brought desulfurization forward. At 400 °C, the #400 mesh sample removed 83% of the sulfur and the #200 mesh sample only 20% (Figure 2a). From 600 °C both exceeded 95%, and at 800 °C the residual sulfur was 0.36–0.41% (Table S1). Arsenic was also partly removed: after 150 min at 600 °C, the calcine contained 0.25% As at #200 mesh and 0.30% at #400 mesh, against 0.53% and 0.50% in the tailing. Corrected for mass loss (22.2% and 20.0%), 63% and 52% of the As was removed, respectively.
At 600 °C, the #400 mesh sample removed 62% of the sulfur in 15 min, against 40% for #200 mesh, and both exceeded 96% at 150 min (Figure 2b). At 400 and 500 °C the mass increased slightly after 60 min; for example, the mass loss of the #400 mesh sample at 400 °C fell from 15.58% to 14.66%.
We estimated the apparent activation energy of roasting from the mass loss in the first 30 min (Table S2). With the shrinking-core model it was 24 ± 3 kJ/mol for #200 mesh and 17 ± 1 kJ/mol for #400 mesh; with the product-layer diffusion model, 44 ± 7 and 30 ± 2 kJ/mol (R² = 0.93–0.99). In both cases the finer size had the lower activation energy.
The XRD patterns show the transformation directly (Figure 3). In the unroasted tailing, the pyrite reflections (33.0°, 37.1°, 40.8°, 47.4° and 56.3° 2θ) dominate together with quartz, and melanterite appears at 18.1°. At #200 mesh, pyrite still dominated at 400 °C, whereas at #400 mesh its reflections had almost disappeared and maghemite and hematite had formed. At 500 °C, maghemite and hematite coexisted at both sizes, and from 600 °C only hematite and quartz remained as major phases, with hematite reflections becoming more intense at 700–800 °C.
The distribution of iron among phases, calculated from the sulfur balance and the XRD proportions (Figure 4), shows the sequence pyrite → magnetite/maghemite → hematite. In the unroasted tailing, 92–93% of the Fe is in pyrite, equivalent to about 58% pyrite in the tailing, in agreement with the normative composition. At #200 mesh and 400 °C, 82% of the Fe was still in pyrite and the rest had converted to magnetite. At 500 °C maghemite and hematite dominated, although about 10% of the Fe remained as pyrite, which matches the pyrite cores seen by SEM. From 700 °C practically all the Fe was hematite. At #400 mesh, only 11% of the Fe remained as pyrite at 400 °C; another 11% was in iron sulfates and the rest in maghemite and hematite, and from 600 °C 99–100% of the Fe was hematite.

3.3. Transformation Textures and Gold Location

Backscattered electron images show that pyrite oxidizes from the rim toward the center (Figure 5). At 400 °C, the #200 mesh pyrite kept its shape, with a thin oxide sub-rim. At 500 °C, pyrite cores surrounded by concentric oxide rims were observed, with 10–50% of pyrite remaining per particle. At 600 °C, porous pyrrhotite relics appeared within the oxide pseudomorphs, and at 700–800 °C oxide pseudomorphs with random porosity and scarce pyrrhotite relics dominated. At the SEM scale, the oxides at 800 °C do not look more compact than at 600 °C.
At 400 °C the difference between particle sizes is evident (Figure 5g,h). At #200 mesh the sample is nearly intact pyrite, whereas at #400 mesh all metallic particles are porous iron oxides. At 800 °C and #400 mesh, the oxides showed a graphic texture, with semi-quantitative contents of up to 7.5% Zn and 0.7% Cu, and residual pyrite was found only as inclusions of up to 7 µm within quartz grains.
Gold changed position with roasting (Figure 6). At 400–500 °C and #200 mesh it appeared encapsulated in the still-unoxidized pyrite; at 800 °C a gold grain of about 8 µm was observed within the pores of the iron oxide. This is a single observation: it may be an originally larger grain or the result of coalescence of fine grains during roasting, and our data cannot distinguish between the two.

3.4. Au and Ag Extraction

Roasting increased gold extraction 3.7-fold, with a maximum of 52.7% at 600 °C and #400 mesh, compared with 14.2% unroasted (Figure 7). At #200 mesh, Au extraction remained between 36% and 38% from 400 to 600 °C. Both sizes dropped to 25–27% at 800 °C. Silver peaked at 600 °C (46.4% at #200 mesh and 37.7% at #400 mesh). All balances except Au at #400 mesh and 700 °C (6.2 points) met the criterion of less than 5 points between calculated and assayed extraction (Table S3). That case was kept in the analysis with the calculated extraction, which is used throughout this work.
Dissolution was fast: by 12 h, 78–94% of the gold obtained at 72 h had already been extracted (Figure 8). The ANOVA (Table 2) showed that temperature explains 68% of the variability in Au extraction and 90% in Ag extraction. The particle size × temperature interaction was the second most important effect for both metals. Particle size was significant for Au (p < 0.001) but not for Ag (p = 0.324), and the temperature × time interaction was not significant for Au (p = 0.700).

3.5. Metal Balance and Cyanide Consumption

Au retention in the calcines was 95.5–99.7% at #200 mesh and 81.7–92.6% at #400 mesh; Ag showed similar values (Table S4). Referred to the original tailing, overall Au recovery was 48.8% under the best condition (#400 mesh, 600 °C), equivalent to about 1.1 g Au and 19 g Ag per tonne of tailing (based on head grades of 2.34 g/t Au and 58.3 g/t Ag for the #400 mesh tailing). NaCN consumption was 22.8–43.6 kg/t for the calcines and 30.5–35.8 kg/t for the unroasted tailing. The lowest values corresponded to 600 °C at #400 mesh (27.3 kg/t) and to 800 °C (22.8–26.8 kg/t).

4. Discussion

4.1. Why the Gold Is Refractory and How Roasting Releases It

The first key result is that the refractoriness of this tailing is not due to poor pyrite liberation, which exceeds 99%, but to the gold being inside the pyrite. As long as the pyrite remains intact, cyanide cannot reach the ~2 µm gold inclusions or the Ag–Au tellurides, which is why direct cyanidation does not exceed 14%. This is the same behavior as refractory pyritic concentrates, whose extraction without pretreatment is usually below 50% [13,14,15] (Table S5), and it is consistent with the presence of tellurides [17,18]. For a tailing, this has a practical consequence: finer grinding is not enough; the pyrite must be destroyed.
The images in Figure 5 show how this destruction takes place. Pyrite does not oxidize all at once. An oxide rim first forms at the edge and advances toward the center, leaving an ever-smaller sulfide core, as described by the shrinking-core model [21]. The pyrrhotite relics at 600 °C and the maghemite detected at 400–500 °C confirm that the reaction passes through intermediate phases before reaching hematite [22,23]. Because particle size is one of the variables that control the rate and pathway of the thermal oxidation of pyrite [22,32], the 38 µm particles oxidize completely at 400 °C, whereas the 75 µm particles barely form a rim. From 600 °C both sizes oxidize fully and the size advantage disappears.
The kinetics support this reading. The apparent activation energies we obtained (17–44 kJ/mol) are far below the 70 kJ/mol reported for the pyrite-to-pyrrhotite conversion in a thermobalance, where chemical reaction is rate-controlling [22]. This indicates that, in the furnace bed, the rate is controlled mainly by the transport of O₂ and SO₂ between particles and through the oxide layer. This is why fine grinding, which shortens these paths, lowers the activation energy and brings desulfurization forward.
At 400–500 °C the calcine gained some mass after the first hour. The most likely explanation is that part of the released SO₂ was fixed again on the oxide as iron sulfate. This sulfate, detected by XRD, accounts for the 6.5% sulfur retained by the #400 mesh calcine at 400 °C, even though SEM no longer showed pyrite. Iron sulfates decompose and are removed as the temperature rises, between 550 and 700 °C [33]. Their presence at 400 °C has a cost: they are soluble in the alkaline pulp and consume cyanide [29], which explains why this calcine had one of the highest consumptions (41–43 kg/t).

4.2. Optimum Temperature and the Decline in Extraction at High Temperature

Gold extraction follows the state of the calcine. At 600 °C with fine grinding, three favorable conditions come together: almost all the sulfur is gone (96.6%), no sulfates remain and the hematite is porous. Under this condition, 52.7% of the gold was extracted. The 500–600 °C optimum agrees with that reported for pyrite concentrates [13,24] and with the maximum pore volume of the calcine [14,25,26]. Coronado et al. [24] obtained a very similar result for a refractory gold–silver concentrate: their best condition was also 600 °C, with about 50% Au and 61% Ag. Roasting in air, as in our case, is also the atmosphere that best exposes gold encapsulated in pyrite [27]. The particle size × temperature interaction detected by the ANOVA has a simple reading: fine grinding only helps when the temperature is high enough to oxidize all the sulfide without reaching 800 °C, where extraction falls again.
Why is the maximum extraction from this tailing (53%) lower than that of roasted pyritic concentrates, which reach 80–88% [13,14,34] (Table S5)? Three differences explain it. First, this tailing was roasted as received, without prior concentration: the gold-bearing pyrite, about 58% of the tailing, is accompanied by about 40% quartz, phyllosilicates and sulfates, and the tailing is also more refractory to begin with: unroasted, it yields 13–14% of the gold, against 10–48% for those concentrates, and part of the gold is in tellurides. Measured as a relative gain, roasting increased extraction 3.7-fold, more than in the concentrates of Zhang et al. (3.4-fold) [13] and Espinoza-Martínez et al. (1.7-fold) [34], although less than in that of Mao et al. (8.8-fold) [14]. Second, the tailing carries sulfates and copper minerals that compete for cyanide. Third, we roasted in a static bed, where gas transport controls the rate; in fluidized beds or thin layers, contact with oxygen is much better. A refractory gold–silver concentrate roasted under conditions similar to ours also gave about 50% Au [24]. This suggests that a fluidized-bed roaster could exceed the extraction we obtained in the laboratory.
Above 600 °C, extraction falls to 25–27% at 800 °C. In concentrates, this decline is attributed to the sintering of hematite, which closes the pores and locks the gold again [13,26]. In this tailing, however, SEM did not show clear densification: at 800 °C the oxides are still pseudomorphs with random porosity (Figure 5), and in one of them gold was seen within the pores (Figure 6b). Because porosity was not measured, incipient sintering below the resolution of SEM cannot be ruled out, but it is not the only possible explanation. There are also other factors. The oxides roasted at 800 °C contain up to 7.5% Zn and 0.7% Cu, which suggests the formation of ferrites. Zinc ferrite forms during the oxidative roasting of zinc concentrates [33], and copper ferrites have been observed between 650 and 750 °C in the roasting of silver tailings [35]. These phases are dense, poorly reactive and can trap gold. The silicate gangue also plays a role, although our data can only bound it. According to semi-quantitative XRD, pyrophyllite was no longer detected at 700 °C at #200 mesh and muscovite dropped from 6.5% to 1.4% between 600 and 800 °C, consistent with their dehydroxylation, which occurs between 500 and 900 °C in pyrophyllite [36] and between 700 and 1000 °C in muscovite [37]. In SEM, however, these phyllosilicates still appeared as free particles, with no visible bonding to the iron oxides, so we found no evidence of sintering between gangue and oxides. What was observed in all samples, roasted or not, were quartz grains with inclusions of pyrite or iron oxides; at 800 °C and #400 mesh, residual pyrite was found only as inclusions of up to 7 µm within quartz. That pyrite and the gold it contains remain out of reach of oxygen and cyanide at any temperature, and their relative weight is greater in a tailing than in a concentrate. XRD did not detect fayalite (Fe₂SiO₄) or other iron silicates. Silver follows the same pattern, peaking at 600 °C, in line with the formation of Ag–Fe–S species and silver ferrite that are poorly soluble in cyanide [13].
Figure 9 summarizes the mechanism we propose from the textures, the iron distribution and the extractions.

4.3. Residual Gold, Cyanide Consumption and Mass Losses

Even under the best condition, 47% of the gold remains in the residue. Because extraction levels off by 24 h, this gold is not accessible to cyanide within practical times. In calcines from refractory concentrates, the remaining gold is trapped in iron oxides and silicates, especially in the fine fraction, and alkaline washing or sulfuric acid curing before cyanidation can raise extraction from 70% to 94% [30]. In calcine residues from Zimbabwe, by contrast, almost all the remaining gold was submicroscopic and did not respond to ultrafine grinding [19]. Testing these treatments on our calcine is the natural next step.
Cyanide consumption is the main economic barrier. Even the unroasted tailing consumed 30–36 kg/t NaCN, far above usual industrial values. The cause is copper: the tailing contains 0.36% Cu in tennantite, enargite and chalcopyrite; these minerals, and the copper oxides and sulfates that probably form during roasting (not identified by XRD or SEM), react with cyanide and form copper complexes that consume it [29]. Roasting does not remove this copper: normalized to Fe, Cu retention in the calcines was 1.00–1.17 at all temperatures (Table S6), so the cyanicide stays in the calcine. In other ores, removing copper beforehand with an ammonia pretreatment allowed almost all the gold to be extracted with low reagent consumption [28]. Scaling up the process will require evaluating that pretreatment, washing of the calcine [30] and a lower NaCN concentration.
The #400 mesh calcines retained between 82% and 93% of their Au and Ag. To determine whether this loss was physical or due to volatilization, we used iron as a tracer, since it does not volatilize at these temperatures. Normalized to Fe, the retention of Au and Ag was 1.01 to 1.16 under all conditions (Table S6); that is, gold and silver were lost in the same proportion as iron. The loss was therefore physical: fine particles carried away when the bed was stirred. Zn and Cu were also retained in the same proportion as Fe, consistent with their incorporation into the iron oxides. The only metal with a clear relative loss was Pb at 800 °C and #200 mesh (about 16% relative to Fe), which suggests partial volatilization and should be considered in emission control. In an industrial roaster, the entrained fines would be recovered in the dust collection system; in the laboratory, recovery should be reported relative to the original tailing (Table S4), as we have done here.

4.4. Environmental and Process Implications

Roasting also solves part of the environmental problem. At 600 °C, the sulfur in the tailing drops from 32.9% to less than 1.5%; in other words, the pyrite, the main source of acidity, is removed [8,9]. Confirming with static acid–base accounting tests that the calcine is no longer reactive is the next step to close this argument. The cyanidation residue, made up mainly of hematite and quartz, could be used as a source of iron [38], and gold-bearing pyrite cinders have already been treated to recover several metals at once [39]. The process has environmental costs that should not be hidden. It generates SO₂, which must be captured, and it can mobilize arsenic, which reaches 0.5% in this tailing, from arsenopyrite, tennantite and arsenian pyrite. In oxidative roasting, about half of the arsenic can report to the dust [40], and in this work 52–63% of it left the calcine at 600 °C, so the roaster off-gas and dust must be treated. At the Giant mine roasting left arsenic in mobile forms in the tailings [41]. Hydrometallurgical alternatives therefore remain an option for comparison [20].
These results also show how the process should be scaled up. Roasting the whole tailing is technically feasible: it removes almost all the sulfur and increases gold extraction 3.7-fold. But it requires heating to 600 °C about 40% gangue that contains no gold and only absorbs heat, and the final extraction (53%) remains far below that of concentrates (Table S5). The tailing, on the other hand, lends itself well to prior concentration. At the coarse grind (60% −75 µm), its pyrite is already 99.2% liberated according to SEM particle counting, so pyrite flotation would not require fine regrinding; pyrite flotation has already been applied to copper tailings [7]. Because the gold is inside the pyrite, a pyrite concentrate would reduce the mass fed to the roaster by about 40% and could raise the gold grade of the feed up to about 1.7 times, if all the gold reports to the concentrate. We therefore propose a flotation–roasting–cyanidation flowsheet, which we are evaluating in an ongoing study.

4.5. Limitations

This study has several limitations. XRD and SEM particle counting are semi-quantitative. Arsenic in the calcines was analyzed only at 600 °C (150 min), with a technique different from that used for the tailing, and the off-gas and dust were not analyzed. Ferrites and sulfates could not be confirmed: the EDS compositions are semi-quantitative, the spectra are not available, and they do not show which phase hosts the Zn, and in XRD the zinc ferrite peaks overlap with those of magnetite and maghemite. Roasting was carried out in a static muffle furnace, and sulfur was assayed once per condition, so the roasting results are descriptive. Cyanidation was not replicated: each combination of condition and time is a single bottle, so the ANOVA error was estimated from the three-way interaction. In addition, the whole tailing was roasted without concentrating the pyrite, and the surface area and porosity of the calcines were not measured, so incipient sintering at 800 °C cannot be ruled out.

5. Conclusions

  • The refractoriness of the Santa Catalina tailing is not due to poor pyrite liberation (99.2–100%) but to gold locked inside the pyrite: SEM found no free gold and detected ~2 µm gold and Ag–Au tellurides within the residual pyrite of the 400–500 °C calcines; as a result, direct cyanidation extracts only 13–14% of the gold.
  • Roasting oxidizes pyrite from the rim to the center, through pyrrhotite and magnetite/maghemite to porous hematite. Grinding to 95% −38 µm brings desulfurization forward by about 100 °C and lowers the apparent activation energy, indicating that gas transport controls the rate in the bed.
  • The best condition was 600 °C with 95% −38 µm: 96.6% desulfurization and 52.7% Au and 37.7% Ag extraction, with one of the lowest NaCN consumptions (27.3 kg/t). Temperature explained 68% of the variation in gold extraction. At 800 °C, extraction falls to 25–27%, probably because of the formation of Zn and Cu ferrites; SEM did not show clear oxide densification.
  • Au and Ag losses from the fine calcines were physical (entrainment of fines), not due to volatilization; only Pb showed partial volatilization at 800 °C.
  • Roasting the whole tailing is feasible but inefficient. Since the pyrite is already liberated at a coarse grind, it should first be concentrated by flotation and only the concentrate roasted, while controlling cyanide consumption by copper. In this way, the tailing can change from a source of acid drainage into a source of gold and silver.

Supplementary Materials

The following supporting information can be downloaded at the website of this paper posted on Preprints.org, Figure S1: Grinding curve and verification grinds; Table S1: Mass loss, residual sulfur and desulfurization; Table S2: Apparent activation energy of roasting; Table S3: Calculated and assayed extraction and NaCN consumption; Table S4: Metal retention and overall recovery; Table S5: Comparison with the literature; Table S6: Fe-normalized metal retention; Dataset S1: Experimental data (Excel workbook).

Author Contributions

Conceptualization, J.A.V.-G.; methodology, H.R.P.-R.; software, J.A.V.-G. and H.R.P.-R.; formal analysis, H.R.P.-R., A.L.C.-S. and M.M.M.-R.; investigation, J.M.H.-S., A.M.V.-R., D.H.C.-F., A.L.C.-S. and M.M.M.-R.; resources, J.M.H.-S., A.M.V.-R., D.H.C.-F., A.L.C.-S. and M.M.M.-R.; data curation, J.A.V.-G. and H.R.P.-R.; writing—original draft preparation, J.A.V.-G.; writing—review and editing, all authors; visualization, J.A.V.-G. and H.R.P.-R.; supervision, J.A.V.-G.; project administration, J.A.V.-G.; funding acquisition, J.A.V.-G., A.L.C.-S. and L.E.V.-R. All authors have read and agreed to the published version of the manuscript.

Funding

This research was funded by the National Council of Science, Technology and Technological Innovation of Peru (CONCYTEC), through the National Program for Scientific Research and Advanced Studies (PROCIENCIA), under contract No. PE501086389-2024. The APC was funded by PROCIENCIA.

Institutional Review Board Statement

Not applicable.

Data Availability Statement

The data supporting this study are included in the article, its Supplementary Materials and Dataset S1, which contains the grinding verification, roasting mass loss and sulfur data, arsenic data, bottle-roll head and residue assays, solution analyses and the raw XRD patterns. The SEM report (Technical Report No. 007-2024-INGEMMET/DL-LP) and the Python scripts that generate the figures and calculations are available from the corresponding author upon reasonable request.

Acknowledgments

The authors gratefully acknowledge the Geological, Mining and Metallurgical Institute (INGEMMET) and the GEOMETAMB Research Group at the National University of Trujillo for their support in the analytical testing and for providing access to laboratory facilities. During the preparation of this manuscript, the authors used Claude Opus 5.5 (Anthropic, San Francisco, CA, USA) for support with coding the statistical analysis and figures, literature searching, and drafting and translating the text into English, as detailed in Section 2.6. The authors have reviewed and edited the output and take full responsibility for the content of this publication.

Conflicts of Interest

The authors declare no conflicts of interest. The funders had no role in the design of the study; in the collection, analyses, or interpretation of data; in the writing of the manuscript; or in the decision to publish the results.

References

  1. Kossoff, D.; Dubbin, W.E.; Alfredsson, M.; Edwards, S.J.; Macklin, M.G.; Hudson-Edwards, K.A. Mine Tailings Dams: Characteristics, Failure, Environmental Impacts, and Remediation. Appl. Geochem. 2014, 51, 229–245. [Google Scholar] [CrossRef]
  2. Ministerio de Energía y Minas. Resolución Ministerial N.° 335-2022-MINEM/DM: Aprueban la Actualización del Inventario de Pasivos Ambientales Mineros. Diario Oficial El Peruano. 9 September 2022. Available online: https://busquedas.elperuano.pe/dispositivo/NL/2103488-1.
  3. Araujo, F.S.M.; Taborda-Llano, I.; Nunes, E.B.; Santos, R.M. Recycling and Reuse of Mine Tailings: A Review of Advancements and Their Implications. Geosciences 2022, 12, 319. [Google Scholar] [CrossRef]
  4. Kinnunen, P.; Karhu, M.; Yli-Rantala, E.; Kivikytö-Reponen, P.; Mäkinen, J. A Review of Circular Economy Strategies for Mine Tailings. Clean. Eng. Technol. 2022, 8, 100499. [Google Scholar] [CrossRef]
  5. Falagán, C.; Grail, B.M.; Johnson, D.B. New Approaches for Extracting and Recovering Metals from Mine Tailings. Miner. Eng. 2017, 106, 71–78. [Google Scholar] [CrossRef]
  6. Godirilwe, L.L.; Haga, K.; Altansukh, B.; Takasaki, Y.; Ishiyama, D.; Trifunovic, V.; Avramovic, L.; Jonovic, R.; Stevanovic, Z.; Shibayama, A. Copper Recovery and Reduction of Environmental Loading from Mine Tailings by High-Pressure Leaching and SX-EW Process. Metals 2021, 11, 1335. [Google Scholar] [CrossRef]
  7. Valderrama, L.I.; Santander, M.E. Recovery of Pyrite from Copper Tailings by Flotation. J. Mater. Res. Technol. 2019, 8, 4312–4317. [Google Scholar] [CrossRef]
  8. Akcil, A.; Koldas, S. Acid Mine Drainage (AMD): Causes, Treatment and Case Studies. J. Clean. Prod. 2006, 14, 1139–1145. [Google Scholar] [CrossRef]
  9. Nieva, N.E.; Borgnino, L.; García, M.G. Long Term Metal Release and Acid Generation in Abandoned Mine Wastes Containing Metal-Sulphides. Environ. Pollut. 2018, 242, 264–276. [Google Scholar] [CrossRef] [PubMed]
  10. Balci, N.; Demirel, C. Prediction of Acid Mine Drainage (AMD) and Metal Release Sources at the Küre Copper Mine Site, Kastamonu, NW Turkey. Mine Water Environ. 2018, 37, 56–74. [Google Scholar] [CrossRef]
  11. Huaranga Moreno, F.; Méndez García, E.; Quilcat León, V.; Huaranga Arévalo, F. Pollution by Heavy Metals in the Moche River Basin, 1980–2010, La Libertad—Peru. Sci. Agropecu. 2012, 3, 235–247. [Google Scholar] [CrossRef]
  12. Espinoza, S.N.A.; Mostacero, L.J.S.; Espinoza, A.V.V.; Aguilar, C.E.del C. Crecimiento Exponencial de la Contaminación del Río Moche. SCIÉNDO 2024, 27, 53–58. [Google Scholar] [CrossRef]
  13. Zhang, Y.-P.; Yang, K.; Fang, Y.; Robledo-Cabrera, A.; Peng, C.-S.; Lopez-Valdivieso, A. Roasting Temperature Effect on the Recovery of Refractory Gold and Silver in Pyrite Concentrates. J. Min. Metall. Sect. B-Metall. 2021, 57, 235–243. [Google Scholar] [CrossRef]
  14. Mao, Y.; Ying, H.; Yang, Y.; Liu, M.; Li, X. Influence of Oxidation Roasting on Pore Structure Evolution and Gold Extraction in Refractory Gold Concentrate. Minerals 2026, 16, 902. [Google Scholar] [CrossRef]
  15. Guner, M.K.; Bulut, G.; Hassanzadeh, A.; Lode, S.; Aasly, K. Automated Mineralogy and Diagnostic Leaching Studies on Bulk Sulfide Flotation Concentrate of a Refractory Gold Ore. Minerals 2023, 13, 1243. [Google Scholar] [CrossRef]
  16. Alfonso, P.; Anticoi, H.; Yubero, T.; Bascompta, M.; Henao, L.; Garcia-Valles, M.; Palacios, S.; Yáñez, J. The Importance of Mineralogical Knowledge in the Sustainability of Artisanal Gold Mining: A Mid-South Peru Case. Minerals 2019, 9, 345. [Google Scholar] [CrossRef]
  17. Zhang, J.; Zhang, Y.; Richmond, W.; Wang, H. Processing Technologies for Gold-Telluride Ores. Int. J. Miner. Metall. Mater. 2010, 17, 1–10. [Google Scholar] [CrossRef]
  18. Yang, W.; Cao, H.; Wang, Y.P.; Long, T.; Wan, H.; Li, H.; Dong, P. Dissolution Kinetics of Tellurium from Gold Concentrate during Alkaline Sulphide Leaching. J. S. Afr. Inst. Min. Metall. 2019, 119, 883–890. [Google Scholar] [CrossRef]
  19. Bare, G.T.; Mbayo, J.J.K.; Ndlovu, S.; Shemi, A.; Chipise, L. Mineralogical Characterization and Acid Pretreatment of a Gold Calcine Leach Residue. Minerals 2022, 12, 10. [Google Scholar] [CrossRef]
  20. Wang, S.; Wu, J.; Jiao, F. Pretreatment and Extraction of Gold from Refractory Gold Ore in Acidic Conditions. Minerals 2025, 15, 340. [Google Scholar] [CrossRef]
  21. Zhang, Y.; Li, Q.; Liu, X.; Xu, B.; Yang, Y.; Jiang, T. A Thermodynamic Analysis on the Roasting of Pyrite. Minerals 2019, 9, 220. [Google Scholar] [CrossRef]
  22. Aracena, A.; Jerez, O. Mechanism and Kinetics of Pyrite Transformation at Elevated Temperatures. Physicochem. Probl. Miner. Process. 2021, 57, 127–139. [Google Scholar] [CrossRef]
  23. Music, S.; Popović, S.; Ristić, M. Thermal Decomposition of Pyrite. J. Radioanal. Nucl. Chem. 1992, 162, 217–226. [Google Scholar] [CrossRef]
  24. Coronado, J.H.; Encinas, M.A.; Leyva, J.C.; Valenzuela, J.L.; Valenzuela, A.; Munive, G.T. Roasting of Refractory Gold and Silver Concentrate. Rev. Metal. 2012, 48, 165–174. [Google Scholar] [CrossRef]
  25. Li, H.; Li, Z.; Jin, J.; Han, Y.; Li, Y. Pore Evolution in Refractory Gold Ore Formed by Oxidation Roasting and the Effect on the Cyanide Leaching Process. ACS Omega 2022, 7, 3618–3625. [Google Scholar] [CrossRef] [PubMed]
  26. Xiao, H.; Wei, S.; Li, H.; Zhao, L.; Ma, S.; Luo, S. Fluidized Roasting of Carbonaceous Gold Ore in O₂/CO₂ Atmosphere: Effects of Temperature on Gold Leaching and Mineralogical Transformations. Minerals 2026, 16, 908. [Google Scholar] [CrossRef]
  27. Larachi, F.; Lukumu, D.B.; Baş, A.D. Susceptibility to Cyanidation of Pyrrhotite-Associated Gold in Pyrite Calcines from (Non)Oxidizing Roasting Environments. Miner. Eng. 2023, 202, 108245. [Google Scholar] [CrossRef]
  28. Bas, A.D.; Koc, E.; Yazici, E.Y.; Deveci, H. Treatment of Copper-Rich Gold Ore by Cyanide Leaching, Ammonia Pretreatment and Ammoniacal Cyanide Leaching. Trans. Nonferrous Met. Soc. China 2015, 25, 597–607. [Google Scholar] [CrossRef]
  29. Kianinia, Y.; Khalesi, M.R.; Abdollahy, M.; Hefter, G.; Senanayake, G.; Hnedkovsky, L.; Darban, A.K.; Shahbazi, M. Predicting Cyanide Consumption in Gold Leaching: A Kinetic and Thermodynamic Modeling Approach. Minerals 2018, 8, 110. [Google Scholar] [CrossRef]
  30. Li, Q.; Zhang, Y.; Liu, X.; Xu, B.; Yang, Y.; Jiang, T. Improvement of Gold Leaching from a Refractory Gold Concentrate Calcine by Separate Pretreatment of Coarse and Fine Size Fractions. Minerals 2017, 7, 80. [Google Scholar] [CrossRef]
  31. Velásquez-Ríos, A.M.; Cortez-Flores, D.H. Influencia de la Temperatura de Tostación y Granulometría en la Extracción de Oro Mediante Cianuración del Relave Santa Catalina—La Libertad. Undergraduate Thesis, Universidad Nacional de Trujillo, Trujillo, Peru, 2025. Available online: https://repositorio.unitru.edu.pe/entities/publication/cc037a41-30e8-48b6-b871-848cf218bc8e.
  32. Hu, G.; Dam-Johansen, K.; Wedel, S.; Hansen, J.P. Decomposition and Oxidation of Pyrite. Prog. Energy Combust. Sci. 2006, 32, 295–314. [Google Scholar] [CrossRef]
  33. Grudinsky, P.; Pankratov, D.; Kovalev, D.; Grigoreva, D.; Dyubanov, V. Comprehensive Study on the Mechanism of Sulfating Roasting of Zinc Plant Residue with Iron Sulfates. Materials 2021, 14, 5020. [Google Scholar] [CrossRef] [PubMed]
  34. Espinoza-Martínez, A.M.; Valenzuela-García, J.L.; Salazar-Campoy, M.M.; Encinas-Romero, M.A.; Martínez-Ballesteros, G.; Parga Torres, J.R. Gold and Silver Recovery from a Refractory Pyritic Concentrate by Roasting and Alkaline Pressure Oxidation. Minerals 2025, 15, 1260. [Google Scholar] [CrossRef]
  35. Chang, J.; Pan, A.; Ma, Y.; Sun, Y.; Hu, S.; Li, K. Thermodynamics and Mechanisms of Silver Tailings Roasting Processes. Metall. Res. Technol. 2022, 119, 114. [Google Scholar] [CrossRef]
  36. Wang, L.; Zhang, M.; Redfern, S.A.T.; Zhang, Z. Dehydroxylation and Transformations of the 2:1 Phyllosilicate Pyrophyllite at Elevated Temperatures: An Infrared Spectroscopic Study. Clays Clay Miner. 2002, 50, 272–283. [Google Scholar] [CrossRef]
  37. Mazzucato, E.; Artioli, G.; Gualtieri, A. High Temperature Dehydroxylation of Muscovite-2M1: A Kinetic Study by in Situ XRPD. Phys. Chem. Miner. 1999, 26, 375–381. [Google Scholar] [CrossRef]
  38. Yang, C.-C.; Zhu, D.-Q.; Pan, J.; Li, S.-W.; Tian, H.-Y. A Novel Process for Fe Recovery and Zn, Pb Removal from a Low-Grade Pyrite Cinder with High Zn and Pb Contents. Int. J. Miner. Metall. Mater. 2018, 25, 981–989. [Google Scholar] [CrossRef]
  39. Ding, J.; Han, P.-W.; Lü, C.-C.; Qian, P.; Ye, S.-F.; Chen, Y.-F. Utilization of Gold-Bearing and Iron-Rich Pyrite Cinder via a Chlorination–Volatilization Process. Int. J. Miner. Metall. Mater. 2017, 24, 1241–1250. [Google Scholar] [CrossRef]
  40. Dosmukhamedov, N.; Kaplan, V.; Zholdasbay, E.; Argyn, A.; Kuldeyev, E.; Koishina, G.; Tazhiev, Y. Chlorination Treatment for Gold Extraction from Refractory Gold-Copper-Arsenic-Bearing Concentrates. Sustainability 2022, 14, 11019. [Google Scholar] [CrossRef]
  41. Walker, S.R.; Jamieson, H.E.; Lanzirotti, A.; Hall, G.E.M.; Peterson, R.C. The Effect of Ore Roasting on Arsenic Oxidation State and Solid Phase Speciation in Gold Mine Tailings. Geochem. Explor. Environ. Anal. 2015, 15, 273–291. [Google Scholar] [CrossRef]
Figure 1. Experimental flowsheet.
Figure 1. Experimental flowsheet.
Preprints 243858 g001
Figure 2. Desulfurization corrected for mass loss: (a) as a function of temperature after 3 h; (b) as a function of time at 600 °C.
Figure 2. Desulfurization corrected for mass loss: (a) as a function of temperature after 3 h; (b) as a function of time at 600 °C.
Preprints 243858 g002
Figure 3. XRD patterns of the tailing and calcines: (a) 60% −75 µm; (b) 95% −38 µm. Patterns are normalized and offset; symbols mark the main reflections of the phases identified in each sample.
Figure 3. XRD patterns of the tailing and calcines: (a) 60% −75 µm; (b) 95% −38 µm. Patterns are normalized and offset; symbols mark the main reflections of the phases identified in each sample.
Preprints 243858 g003
Figure 4. Distribution of iron among phases in the tailing and calcines: (a) 60% −75 µm; (b) 95% −38 µm. The Fe fraction in pyrite and sulfates was calculated from the measured sulfur, and the remaining Fe was split between magnetite/maghemite and hematite according to their XRD proportions. “Other” is the Fe in silicates and base-metal sulfides.
Figure 4. Distribution of iron among phases in the tailing and calcines: (a) 60% −75 µm; (b) 95% −38 µm. The Fe fraction in pyrite and sulfates was calculated from the measured sulfur, and the remaining Fe was split between magnetite/maghemite and hematite according to their XRD proportions. “Other” is the Fe in silicates and base-metal sulfides.
Preprints 243858 g004
Figure 5. Transformation of pyrite observed by SEM (backscattered electrons). Sequence at 60% −75 µm: (a) unroasted, free pyrite (py) and gangue (GGs); (b) 400 °C, iron oxide (OXsFe) sub-rim at the pyrite edge; (c) 500 °C, pyrite core with oxide rim; (d) 600 °C, relict pyrrhotite (po) with voids; (e) 700 °C, porous iron oxide pseudomorph; (f) 800 °C, pseudomorph with scarce pyrrhotite relics. Effect of particle size at 400 °C: (g) 60% −75 µm, nearly intact pyrite with sphalerite (ef) and gangue; (h) 95% −38 µm, porous iron oxide particles next to quartz (cz). Images from the INGEMMET Petromineralogy Laboratory; labels follow the laboratory’s Spanish abbreviations.
Figure 5. Transformation of pyrite observed by SEM (backscattered electrons). Sequence at 60% −75 µm: (a) unroasted, free pyrite (py) and gangue (GGs); (b) 400 °C, iron oxide (OXsFe) sub-rim at the pyrite edge; (c) 500 °C, pyrite core with oxide rim; (d) 600 °C, relict pyrrhotite (po) with voids; (e) 700 °C, porous iron oxide pseudomorph; (f) 800 °C, pseudomorph with scarce pyrrhotite relics. Effect of particle size at 400 °C: (g) 60% −75 µm, nearly intact pyrite with sphalerite (ef) and gangue; (h) 95% −38 µm, porous iron oxide particles next to quartz (cz). Images from the INGEMMET Petromineralogy Laboratory; labels follow the laboratory’s Spanish abbreviations.
Preprints 243858 g005
Figure 6. Gold location at 60% −75 µm (SEM): (a) native gold (Au) included in pyrite at 500 °C; (b) gold grain of about 8 µm in the pores of the iron oxide at 800 °C.
Figure 6. Gold location at 60% −75 µm (SEM): (a) native gold (Au) included in pyrite at 500 °C; (b) gold grain of about 8 µm in the pores of the iron oxide at 800 °C.
Preprints 243858 g006
Figure 7. Extraction at 72 h of (a) Au and (b) Ag as a function of roasting temperature. Dashed lines indicate the unroasted tailing.
Figure 7. Extraction at 72 h of (a) Au and (b) Ag as a function of roasting temperature. Dashed lines indicate the unroasted tailing.
Preprints 243858 g007
Figure 8. Au extraction kinetics for (a) 60% −75 µm and (b) 95% −38 µm. Each point corresponds to an independent bottle.
Figure 8. Au extraction kinetics for (a) 60% −75 µm and (b) 95% −38 µm. Each point corresponds to an independent bottle.
Preprints 243858 g008
Figure 9. Proposed mechanism for gold release during roasting of the tailing and its decline at 800 °C. Unroasted, the gold is locked in pyrite. At 400 °C, the 75 µm particle only forms an oxide rim and exposes the gold near the edge, whereas the 38 µm particle oxidizes completely but retains sulfates. At 600 °C both are porous hematite with exposed gold. At 800 °C the oxide is still porous at the SEM scale, but extraction falls; the most likely cause is the formation of Zn and Cu ferrites, together with pyrite enclosed in quartz. Percentages are Au extractions measured at 72 h; the dashed box marks the best condition.
Figure 9. Proposed mechanism for gold release during roasting of the tailing and its decline at 800 °C. Unroasted, the gold is locked in pyrite. At 400 °C, the 75 µm particle only forms an oxide rim and exposes the gold near the edge, whereas the 38 µm particle oxidizes completely but retains sulfates. At 600 °C both are porous hematite with exposed gold. At 800 °C the oxide is still porous at the SEM scale, but extraction falls; the most likely cause is the formation of Zn and Cu ferrites, together with pyrite enclosed in quartz. Percentages are Au extractions measured at 72 h; the dashed box marks the best condition.
Preprints 243858 g009
Table 1. Chemical composition of the Santa Catalina tailing (60% −75 µm fraction).
Table 1. Chemical composition of the Santa Catalina tailing (60% −75 µm fraction).
Au (g/t) Ag (g/t) Cu (%) Pb (%) Zn (%) Fe (%) S (%) LOI (%)
2.40 62.1 0.36 0.29 0.76 29.61 32.89 25.17
LOI: loss on ignition.
Table 2. Unreplicated factorial ANOVA of Au and Ag extraction (n = 40 bottles; α = 0.05; error = three-way interaction, 12 df).
Table 2. Unreplicated factorial ANOVA of Au and Ag extraction (n = 40 bottles; α = 0.05; error = three-way interaction, 12 df).
Source df F (Au) p (Au) Contribution Au (%) F (Ag) p (Ag) Contribution Ag (%)
Temperature (T) 4 329.0 < 0.001 68.0 1110.8 < 0.001 89.7
Particle size (M) 1 115.3 < 0.001 6.0 1.06 0.324 0.0
Time (t) 3 55.4 < 0.001 8.6 39.3 < 0.001 2.4
M × T 4 74.2 < 0.001 15.3 83.4 < 0.001 6.7
M × t 3 6.5 0.007 1.0 1.51 0.261 0.1
T × t 12 0.73 0.700 0.5 3.51 0.019 0.8
Error 12 — — 0.6 — — 0.2
R² = 0.994 (Au) and 0.998 (Ag). The residual standard deviation of the model, which estimates the experimental error, was 1.0 percentage points for Au and 0.85 for Ag, far smaller than the differences between temperatures.
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.
Copyright: This open access article is published under a Creative Commons CC BY 4.0 license, which permit the free download, distribution, and reuse, provided that the author and preprint are cited in any reuse.