Influence of Heat Input Variation on the Metallurgical Features of the Heat-Affected Zone in API 5L X65 Welded Joints

Submitted:

10 November 2026

Posted:

11 November 2026

You are already at the latest version

Abstract
Understanding the influence of heat input on the microstructural evolution of welded pipeline steels is essential for ensuring mechanical integrity and operational reliability. In this study, the effects of different heat inputs on the microstructural transformations in buttered joints of API 5L X65 PSL2 steel welded by robotic Gas Metal Arc Welding (GMAW) were evaluated. The process was carried out using a shielding gas mixture of 85% Ar and 15% CO₂ with pulsed metal transfer, employing three heat input levels, 0.8, 0.9, and 1.0 kJ.mm⁻¹, classified as low, medium, and high, respectively. A buttering layer was deposited on one side of a half-V groove to generate a linear thermal-affected region using the same welding parameters. Microstructural characterization was performed through optical and scanning electron microscopy, complemented by X-ray diffraction to detect brittle phases formed during thermal cycling. Vickers microhardness measurements HV(0.1) were conducted across three regions of the welds. Results indicated that higher heat input produced a wider thermally altered region. Martensite was detected in the coarse-grained area under all conditions, contributing to increased hardness values. In contrast, regions subjected to intercritical and subcritical cycles exhibited lower hardness due to tempering effects and reduced phase transformation.
Keywords: 
;  ;  ;  ;  

1. Introduction

The American Petroleum Institute (API) is the leading regulatory and technical authority within the oil and natural gas industry, responsible for developing standards and specifications applicable to materials, processes, and transportation systems. The API 5L Specification establishes the technical requirements for line pipes used in oil and gas pipelines, encompassing high-strength low-alloy (HSLA) steels designed for severe service conditions and high structural reliability (API, 2018).
API 5L steels, particularly grades X65 and above, are widely used in pipeline networks for oil and natural gas transportation, as well as in pressure vessels, due to their excellent combination of mechanical strength, toughness, and weldability (Oyyaravelu et al., 2016; Wang et al., 2024). Welding plays a crucial role in the manufacturing of these structures; however, the imposed thermal cycles often cause significant microstructural heterogeneities, especially within the heat-affected zone (HAZ), where localized variations in temperature, composition, and grain size occur (Buzzatti et al., 2022).
During welding, rapid heating and cooling promote redistribution of carbon and alloying elements within the austenite, which may result in the formation of carbon-rich microconstituents such as martensite and bainite in specific regions of the HAZ. When present in excessive amounts, these constituents increase local hardness and decrease toughness, promoting the initiation of cracks and embrittlement (Neumann et al., 2024). Nonetheless, recent studies have demonstrated that the controlled presence of martensite is not necessarily detrimental, provided that its volume fraction, morphology, and relative hardness are properly balanced (Mohammadijoo et al., 2018; Zhang et al., 2012; Keehan et al., 2010).
The prior austenite grain size, determined by the peak temperature reached during welding, has a direct influence on phase transformations and the hardness profile across the HAZ. Works by Digheche et al. (2017) and Wang et al. (2025) reported that increasing heat input generally reduces hardness and promotes coarser microstructures with lower martensite fractions, which can compromise the overall toughness of the welded joint.
In this context, the present study aimed to evaluate the effect of three distinct heat input levels on the microstructural characteristics and microhardness profiles of different HAZ regions in welded joints of API 5L X65 steel. The samples were produced by robotic GMAW (Gas Metal Arc Welding) using pulsed arc metal transfer mode and a shielding gas mixture of 85% Ar + 15% CO₂. The analysis of phase transformations and local properties enabled the correlation between the imposed thermal conditions, the formation of microconstituents, and the hardness variation throughout the HAZ, contributing to a deeper understanding of the microstructural mechanisms governing the mechanical performance of these welded joints.

2. Materials and Methods

2.1. Material

The material investigated was an API 5L X65 PSL2 steel plate supplied by a steel industry (Brazil). Its chemical composition was determined by atomic absorption spectroscopy, using the average of five measurements.

2.2. Welding Equipment

All welding procedures were performed using a Panasonic TM-1400WGIII robotic system, equipped with a six-axis manipulator and an inverter-based power source (350 A). Process control was conducted through a Teach Pendant. This setup ensured high repeatability in the deposition conditions.

2.3. Welding Procedure

2.3.1. General Conditions

Plates with dimensions of 100.0 × 50.0 × 7.4 mm were welded using the MAG process with pulsed DC and reverse polarity (DC+). Three heat inputs were applied: 8 kJ.cm⁻¹ (low), 9 kJ.cm⁻¹ (medium), and 10 kJ.cm⁻¹ (high). The welding speed was kept constant at 21 cm.min⁻¹, and current/voltage were adjusted automatically to maintain arc stability. A solid ER70S-6 wire (1.2 mm) and a shielding gas mixture of 85% Ar / 15% CO₂ at 15 L.min⁻¹ were used.

2.3.2. Buttering Layer

A buttering layer was deposited on one side of the joint to obtain a controlled and nearly linear heat-affected zone (HAZ), enabling later fracture-toughness assessments. Deposition was performed with robotic weaving to ensure uniform filling across the plate thickness. After welding, the buttered surface was machined to prepare the joint bevel.

2.3.3. Joint Welding

Joints were welded in the flat position (1G) using a 4 mm root opening, a 2 mm land, and a 40° half-V bevel. A carbon-steel backing bar was employed. Two passes were required in all conditions: a straight first pass followed by a weaving second pass.

2.4. Metallographic Characterization

Macro- and microstructural examinations were performed on the as-received material and welded samples. Standard grinding and polishing procedures were applied, followed by etching with 3% Nital for microstructural revelation. Optical microscopy (OM) was used to characterize the base metal and HAZ, while scanning electron microscopy (SEM) provided higher-resolution evaluation of microconstituents. Phase quantification in the base metal followed the grid-intercept method (ASTM E112).

2.5. X-Ray Diffraction

X-ray diffraction (XRD) analyses were conducted to identify phases present within the HAZ. Measurements were performed using a Bruker D8 ADVANCE diffractometer with Cu-Kα radiation, scanning from 20° to 80° (2θ). Phase identification was carried out using DIFFRAC.EVA software.

2.6. Hardness Testing

Microhardness measurements (HV0.1) were performed along three transverse lines, upper, mid-thickness, and lower, following the API 5L recommendations for welded joints. Indentations were spaced 0.25 mm apart, covering the transition from base metal to weld metal. The hardness of the as-received steel was also measured (Rockwell B), and values were converted to Vickers hardness according to ASTM E140.

3. Results and Discussion

3.1. Characterization of the Base Metal

3.1.1. Chemical Composition

The chemical composition of the base metal (API 5L X65) was determined by atomic absorption spectroscopy (Table 1). The steel primarily consists of ~ 97.98 wt% Fe, with microalloying additions: C ≈ 0.126 wt%, Mn ≈ 1.416 wt%, Nb ≈ 0.0765 wt%, Ti ≈ 0.0198 wt%, and minor Cu, Al, etc. Carbon equivalent indices (CEIIW ≈ 0.3673; CEPCM ≈ 0.2051) remain within the PSL2 specification, ensuring weldability and controlling hardenability.

3.1.2. Metallography

Optical microscopy of the as-received base metal shows fine-grained ferritic structure with dispersed pearlite. Non-metallic inclusions appear as globular oxides (Figure 1). Quantitative metallography performed on three micrographs revealed approximately 83.5 vol% ferrite and 16.5 vol% pearlite (Table 2). Sparse dark precipitates, likely Nb-rich carbides, are observed within ferritic grains, attributed to microalloying additions that hinder austenite grain growth during hot work.

3.1.3. Hardness

Microhardness measurements (n = 10) on the as-received BM yielded: HRB: 96.2 ± 0.92 and HV(0.1): 217.2 ± 5.5. These baseline hardness values serve as references for comparison with welded zones.

3.2. Weld Joint Characterization

3.2.1. Macrostructure

Cross-sectional macrographs of three weld conditions (low, medium, high heat input: LH, MH, HH) etched with 2% Nital (Figure 2) reveal the influence of heat input on geometry. Notably, the width of the Heat-Affected Zone (HAZ) and the buttering or intermediate layer vary: In the MH sample, reduced deposition led to narrower intercritically transformed HAZ (IC-HAZ) and fine-grained HAZ widths. A recrystallized zone appears between first and second passes in all samples, suggesting repeated thermal cycling recrystallizes the buttering layer.

3.2.2. Microstructure

In the Thermally Affected Zone (TAZ) generated by buttering, micrographs (500×) show two distinct sub-regions (Figure 3 and Figure 4): Coarse-grained region (CG-HAZ): predominately ferrite with equiaxed and acicular morphologies; minor eutectoid carbides (M/A constituents) precipitated at grain boundaries. Fine-grained region (FG-HAZ): more refined equiaxed ferrite, fewer large precipitates.
The grain size tends to increase at higher heat inputs, consistent with grain growth mechanisms driven by thermal cycles. This trend aligns with observations in recent literature: for instance, high-efficiency submerged arc welding studies show microstructural coarsening and increased size of martensite/austenite (M/A) constituents as heat input increases (Li et al., 2023).

3.2.3. Width of HAZ / Intercritically Transformed Zone (IC-HAZ)

Using ImageJ® and correlating with microhardness profiling, the average widths of the intercritical and coarse-grained HAZ zones were measured (Table 3). The results show clear dependence on heat input.

3.2.4. X-Ray Diffraction (XRD)

X-ray diffractograms for LH, MH, and HH samples (Figure 5) reveal peaks corresponding to martensite phases in the intercritical HAZ. The presence of retained austenite / martensite-austenite (M/A) constituents after welding suggests incomplete transformation during cooling, likely due to high tempering rates or large prior austenite grains.
The formation of M/A constituents in the coarse and intercritical HAZ has been widely documented as deleterious for toughness: Mohammadijoo et al. (2018) demonstrated that fraction, size, and morphology of M/A islands strongly depend on heat input and directly influence microhardness and local brittleness.

3.2.5. Scanning Electron Microscopy (SEM)

SEM images (Figure 6) at 3000× magnification in the CG-HAZ show bright, planar microconstituents consistent with M/A islands. These features corroborate the XRD results, indicating that retained austenite and martensite form during cooling from high-temperature weld cycles.
The presence of M/A constituents is consistent with earlier studies: their stability and morphology significantly affect mechanical performance, especially toughness.

3.2.6. Microhardness Profiles

Microhardness (Vickers HV0.1) profiles were measured across the weld cross-sections in three distinct paths (upper, central, lower). The average hardness values per region and condition are presented in Table 4.
Hardness decreases when transitioning from the BM to IC-HAZ, most pronounced in the HH condition (22.6 ± 3.3 HV drop), suggesting softening due to thermal overaging or recrystallization. Hardness then increases from IC-HAZ toward FG-HAZ and CG-HAZ, reaching a maximum in CG-HAZ. This is consistent with the presence of martensite and retained austenite, as larger prior austenite grains and slower cooling favor M/A constituent formation. Interestingly, in some regions (e.g., CG-HAZ), the lower heat input (LH) yields slightly higher hardness than MH and HH, possibly due to higher cooling rates and finer microstructural features.
This hardness trend aligns with the behavior reported by Li et al. (2023), who observed that increasing heat input in high-efficiency submerged arc welding leads to coarser M/A constituents, reduced high-angle grain boundaries, and significantly decreased impact toughness. Previous work by Mohammadijoo et al. (2018) also showed that lower heat input tends to promote higher hardness in CG-HAZ, while higher input leads to microstructural coarsening and reduced hardness.

3.2.7. Microstructure Property Correlation and Fracture Risk

The microstructural evolution observed (grain coarsening, M/A island formation) and the hardness distribution suggest that the CG-HAZ is the most critical region for potential embrittlement. The presence of M/A constituents, especially in coarse-grained regions, can act as local brittle zones, reducing toughness by facilitating crack initiation and propagation. This is consistent with well-established understanding in the pipeline-steel literature. For example, in a recent review on micro-alloying effects in HSLA steels, it is highlighted that micro-alloying elements such as Ti, Nb, and V influence the nucleation of intragranular acicular ferrite and thus mitigate the formation of coarse brittle phases in the CG-HAZ (Chen et al., 2025).
Moreover, in the context of hydrogen embrittlement risk, recent studies emphasize that regions with retained austenite and martensite in pipeline steels (such as X65) represent critical weak spots under service conditions. In fact, Chalfoun et al. (2025) demonstrated that fracture resistance of tailored HAZ microstructures (ferritic-bainitic, bainitic, martensitic) under hydrogen is severely reduced, underlining the importance of detailed microstructural control.

3.2.8. Fundamental Mechanisms: Grain Size and Austenite Stability

The increase in grain size observed at higher heat input can be rationalized by thermodynamics and kinetics: larger prior austenite grains have lower boundary density, favoring formation of coarse martensite/austenite islands and reducing grain boundary strengthening. This is supported by studies on lath martensite: Hidalgo and Santofimia (2016) showed that smaller prior austenite grain sizes lead to higher misorientation boundary density and refined martensite, improving mechanical stability. In addition, the thermal and mechanical stability of retained austenite is influenced by the matrix and prior processing: the work of Hidalgo et al. (2017) demonstrated that tempering of the surrounding martensite reduces dislocation density, which in turn lowers the mechanical stability of the retained austenite. These mechanisms are directly relevant to the present findings: the interplay between heat input, grain size, M/A morphology, and cooling rates governs the final microstructure and mechanical performance of the weld.

4. Conclusions

  • Variations in heat input during GMAW significantly influenced the microstructural evolution within the buttered region of API 5L X65 PSL2 welds.
  • The intercritical region (ICHAZ) showed the highest sensitivity to thermal fluctuations, exhibiting partial austenitization and heterogeneous transformation products that directly affected local hardness and mechanical stability.
  • Exposure to subcritical thermal cycles promoted tempering effects, reducing residual stresses and modifying the morphology of martensite-austenite (M/A) constituents, thereby altering the mechanical response.
  • Higher heat input increased grain coarsening and enhanced softening phenomena within both the intercritical and subcritical zones, while lower heat input preserved finer microstructures with improved performance.
  • The interaction between intercritical transformations and subcritical tempering proved critical to defining property gradients across the thermally affected region.
  • These findings reinforce the need for precise optimization of heat input to control microstructural heterogeneity and ensure the structural integrity of welded pipeline steels.

References

  1. API Specification 5L. Specification for Line Pipe, 46th ed.; American Petroleum Institute: Washington, DC, USA, 2018.
  2. Oyyaravelu, R.; Kuppan, P.; Arivazhagan, N. Metallurgical and mechanical properties of laser welded high strength low alloy steel. J. Adv. Res. 2016, 7, 463–472. [Google Scholar] [CrossRef]
  3. Wang, X.; Wang, X.; Xie, Z.; Shang, C.; Liu, Z. Crystallographic study on microstructure evolution and mechanical properties of coarse grained heat affected zone of a 500 MPa grade wind power steel. J. Mater. Res. Technol. 2024, 31, 3921–3934. [Google Scholar] [CrossRef]
  4. Buzzatti, D.T.; Kanan, L.F.; Dalpiaz, G.; Scheid, A.; Kwietniewski, C.E.F. Effect of heat input and heat treatment on the microstructure and toughness of pipeline girth friction welded API 5L X65 steel. Mater. Sci. Eng. A 2022, 833, 142588. [Google Scholar] [CrossRef]
  5. Neumann, M.; Hälsig, A.; Hensel, J. Influence of welding thermal cycles on properties of TMCP and Q&T steels evaluated by thermo-physical simulation. Weld. World 2024, 68, 183–197. [Google Scholar] [CrossRef]
  6. Mohammadijoo, M.; Valloton, J.; Collins, L.; Henein, H.; Ivey, D.G. Characterization of martensite-austenite constituents and micro-hardness in intercritical reheated and coarse-grained heat affected zones of API X70 HSLA steel. Mater. Charact. 2018, 142, 321–331. [Google Scholar] [CrossRef]
  7. Zhang, X.F.; Han, P.; Terasaki, H.; Sato, M.; Komizo, Y. Analytical Investigation of Prior Austenite Grain Size Dependence of Low Temperature Toughness in Steel Weld Metal. J. Mater. Sci. Technol. 2012, 28, 241–248. [Google Scholar] [CrossRef]
  8. Keehan, E.; Zachrisson, J.; Karlsson, L. Influence of cooling rate on microstructure and properties of high strength steel weld metal. Sci. Technol. Weld. Join. 2010, 15, 233–238. [Google Scholar] [CrossRef]
  9. Digheche, K.; Boumerzoug, Z.; Malika, D.; Saadi, K. Influence of heat treatments on the microstructure of welded API X70 pipeline steel. Acta Metall. Slovaca 2017, 23, 72. [Google Scholar] [CrossRef]
  10. Wang, C.; Wei, G.; Shi, X.; Wang, F.; Zhang, S.; Yang, M.; Yan, C.; Li, S. The Effect of Heat Input on the Microstructure and Mechanical Properties of Laser-Backing Welded X80 Steel. Crystals 2025, 15, 359. [Google Scholar] [CrossRef]
  11. Costa, L.M.T.; Melo, G.N.; Castro, N.A.; Buschinelli, J.A. Microstructural characterization of API 5L X65 and X70 steels manufactured by TMCP process. Tecnol. Metal. Mater. Min. 2022, 19, e2511. [Google Scholar] [CrossRef]
  12. Li, J.; Hu, B.; Zhao, L.; Li, F.; He, J.; Wang, Q.; Liu, R. Influence of Heat Input on the Microstructure and Impact Toughness in Weld Metal by High-Efficiency Submerged Arc Welding. Metals 2023, 13, 1217. [Google Scholar] [CrossRef]
  13. Zhu, Z.; Han, J.; Li, H. Influence of heat input on microstructure and toughness properties in simulated CGHAZ of X80 steel manufactured using high-temperature processing. Metall. Mater. Trans. A 2015, 46, 5467–5475. [Google Scholar] [CrossRef]
  14. Chen, J.; Shi, Z.; Luo, X.; Chai, F.; Pan, T.; Feng, G.; Yang, C. Micro-Alloying Effects on Microstructure and Weldability of High-Strength Low-Alloy Steel: A Review. Materials 2025, 18, 1036. [Google Scholar] [CrossRef]
  15. Chalfoun, D.R.; Parker, J.; Gagliano, M.; Martínez-Pañeda, E. Tailored heat treatments to characterise the fracture resistance of critical weld regions in hydrogen transmission pipelines. Int. J. Hydrogen Energy 2025, 192, 152347. [Google Scholar] [CrossRef]
  16. Hidalgo, J.; Santofimia, M.J. Effect of Prior Austenite Grain Size Refinement by Thermal Cycling on the Microstructural Features of As-Quenched Lath Martensite. Metall. Mater. Trans. A 2016, 47, 5288–5301. [Google Scholar] [CrossRef]
  17. Hidalgo, J.; Findley, K.O.; Santofimia, M.J. Thermal and mechanical stability of retained austenite surrounded by martensite with different degrees of tempering. Mater. Sci. Eng. A 2017, 690, 337–347. [Google Scholar] [CrossRef]
Figure 1.  Optical micrograph (50×) showing non-metallic inclusions (globular oxides).(Micrograph of as-received steel matrix with 1000 µm scale bar).
Figure 1.  Optical micrograph (50×) showing non-metallic inclusions (globular oxides).(Micrograph of as-received steel matrix with 1000 µm scale bar).
Preprints 243496 g001
Figure 2.  Macrographs of cross-sections (a-LH, b-MH, c-HH) annotated to show regions of BM, IC-HAZ, FG-HAZ, CG-HAZ, and buttering.(Macrostructure cross-section views with 2 mm scale bars).
Figure 2.  Macrographs of cross-sections (a-LH, b-MH, c-HH) annotated to show regions of BM, IC-HAZ, FG-HAZ, CG-HAZ, and buttering.(Macrostructure cross-section views with 2 mm scale bars).
Preprints 243496 g002
Figure 3.  Optical micrographs (500×) of the coarse-grained region etched with 3% Nital: (a) low heat input (LH), (b) medium heat input (MH), and (c) high heat input (HH).(Micrographs showing CG-HAZ ferrite/carbide structures with 100 µm scale bars).
Figure 3.  Optical micrographs (500×) of the coarse-grained region etched with 3% Nital: (a) low heat input (LH), (b) medium heat input (MH), and (c) high heat input (HH).(Micrographs showing CG-HAZ ferrite/carbide structures with 100 µm scale bars).
Preprints 243496 g003
Figure 4.  Optical micrographs (500×) of the fine-grained region etched with 3% Nital: (a) low heat input (LH), (b) medium heat input (MH), and (c) high heat input (HH).(Micrographs showing FG-HAZ refined ferrite structure with 100 µm scale bars).
Figure 4.  Optical micrographs (500×) of the fine-grained region etched with 3% Nital: (a) low heat input (LH), (b) medium heat input (MH), and (c) high heat input (HH).(Micrographs showing FG-HAZ refined ferrite structure with 100 µm scale bars).
Preprints 243496 g004
Figure 5.  X-ray diffraction patterns of the welded joints produced with (a) low heat input (LH), (b) medium heat input (MH), and (c) high heat input (HH).(Diffraction plots showing intensity vs. 2θ for iron and martensite phases).
Figure 5.  X-ray diffraction patterns of the welded joints produced with (a) low heat input (LH), (b) medium heat input (MH), and (c) high heat input (HH).(Diffraction plots showing intensity vs. 2θ for iron and martensite phases).
Preprints 243496 g005
Figure 6.  SEM micrographs (3000×) of the coarse-grained HAZ etched with 2% Nital: (a) low heat input and (b) high heat input.(SEM images highlighting M-A islands with 2 µm scale bars).
Figure 6.  SEM micrographs (3000×) of the coarse-grained HAZ etched with 2% Nital: (a) low heat input and (b) high heat input.(SEM images highlighting M-A islands with 2 µm scale bars).
Preprints 243496 g006
Table 1. Chemical composition (wt%) of the base metal.
Table 1. Chemical composition (wt%) of the base metal.
Element wt % Element wt %
Fe 97.98 Al 0.0708
C 0.1257 Co <0.005
Si 0.2016 Cu 0.0076
Mn 1.416 Nb 0.0765
P 0.0102 Ti 0.0198
S <0.005 V <0.005
Cr 0.0134 W <0.010
Mo <0.005 Pb <0.005
Ni <0.005 - -
The composition meets the API 5L PSL2 criteria: (i) Nb + V + Ti < 0.15 wt %, (ii) trace element maxima, and (iii) carbon equivalent limits.
Table 2. Phase quantification of base metal.
Table 2. Phase quantification of base metal.
Phase Volume fraction (%)
Ferrite 83.52
Pearlite 16.48
The refined grain structure is consistent with microalloyed TMCP (thermo-mechanically controlled processed) steels: similar to observations reported by Costa et al. (2022), who found quasi-polygonal ferrite with eutectoid aggregates in X65 processed by TMCP.
Table 3. Measured HAZ (IC-HAZ & CG-HAZ) widths for different conditions.
Table 3. Measured HAZ (IC-HAZ & CG-HAZ) widths for different conditions.
Condition Profile (lower, central, upper) Mean HAZ Width (mm)
HH (High) 3.57 / 3.45 / 2.97 ~ 3.33
MH (Medium) 2.85 / 2.79 / 2.06 ~ 2.57
LH (Low) 2.88 / 2.81 / 2.63 ~ 2.77
The largest HAZ occurs at high heat input (HH), consistent with the idea that greater thermal input increases the extent of grain coarsening and transformation zones. Similar behavior was observed in multi-pass welding of HSLA steels (Zhu et al., 2015) where higher heat input broadens coarse-grained regions and increases grain size, negatively affecting toughness.
Table 4. Average microhardness (HV0.1) in different weld regions.
Table 4. Average microhardness (HV0.1) in different weld regions.
Region LH MH HH
BM 226 ± 5.1 229.6 ± 3.6 238.2 ± 1.3
IC-HAZ 198.8 ± 1.2 201.7 ± 1.2 203.9 ± 2.2
FG-HAZ 212.7 ± 2.9 208.9 ± 2.9 211.7 ± 1.4
CG-HAZ 225.4 ± 2.1 222.3 ± 3.7 221.2 ± 1.5
Fusion zone (Weld metal) 226.8 ± 3.8 234.1 ± 2.6 233.5 ± 1.8
 Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.
Copyright: This open access article is published under a Creative Commons CC BY 4.0 license, which permit the free download, distribution, and reuse, provided that the author and preprint are cited in any reuse.