Preprint
Article

This version is not peer-reviewed.

Effects of Heat Input on the Stability of the Sigma Phase in Super Duplex Stainless Steel UNS S32750

Submitted:

10 November 2026

Posted:

11 November 2026

You are already at the latest version

Abstract
Super duplex stainless steels (SDSS) combine excellent mechanical strength and corrosion resistance but may undergo microstructural degradation when exposed to temperatures between 400 and 1010 °C, due to the precipitation of deleterious intermetallic phases such as the sigma (σ) phase. This study investigates the phase evolution in UNS S32750 SDSS subjected to aging treatments at 850, 900, and 950 °C for 10, 100, and 1000 min, followed by water quenching and furnace cooling. The surface and phase microhardness, as well as the volume fraction and average grain size of the σ-phase, were evaluated. The results showed an increase in microhardness with both temperature and aging time, reaching a maximum of 418 ± 4 HV₀.₅ under the 850 °C / 1000 min condition. The σ-phase volume fraction remained nearly constant after 1000 min, regardless of the cooling method, while grain growth exhibited a similar trend across the three evaluated temperatures. These findings enhance the understanding of σ-phase precipitation and dissolution mechanisms and provide valuable insights for defining optimal thermal parameters in welding and manufacturing processes involving UNS S32750 super duplex stainless steel.
Keywords: 
;  ;  ;  ;  ;  

1. Introduction

Technological advances in steel alloy design, combined with the refinement of manufacturing processes, have enabled the widespread adoption of duplex stainless steels (DSS), which are characterized by their simultaneous high mechanical strength and corrosion resistance in aggressive environments. In particular, super duplex stainless steels (SDSS) have gained prominence in critical industrial applications, such as petrochemical, oil and gas (onshore and offshore), and chemical industries, owing to their optimized microstructure and composition, which provide superior performance compared with conventional ferritic and austenitic stainless steels (Francis and Byrne, 2021; Maurya et al., 2024).
These alloys typically exhibit a nearly balanced ferritic–austenitic duplex microstructure, which imparts high toughness, good weldability, and outstanding resistance to localized corrosion. Recent studies have demonstrated that SDSS grades with a Pitting Resistance Equivalent Number (PREN) above 40 show markedly improved resistance to pitting and crevice corrosion relative to standard duplex grades (Pezzato and Calliari, 2022). Moreover, microstructural investigations following heat treatment and welding indicate that maintaining the ferrite/austenite balance and controlling the formation of deleterious precipitates are essential for preserving both mechanical integrity and electrochemical stability (Tütük et al., 2024; Tóth et al., 2024).
Therefore, the main objective of this study is to investigate the phase evolution in a super duplex stainless steel (SDSS), specifically the UNS S32750 grade, subjected to different thermal inputs near the σ-phase dissolution limit. Both computational thermodynamic simulations and experimental thermal analyses were employed to correlate the microstructural transformations with the mechanical and functional behavior of the material. The findings aim to support the establishment of optimized thermal processing parameters that minimize failures associated with the presence of deleterious intermetallic phases.

2. Materials and Methods

2.1. Materials

The super duplex stainless steel (SDSS) UNS S32750 used in this study was extracted from a tube with an outer diameter of 406 mm and a wall thickness of 6 mm. The material was supplied through a collaborative agreement between the Federal University of Espírito Santo (Brazil) and a petrochemical company. The steel was used in the as-received condition (CR) for the preparation of test specimens.

2.2. Specimen Preparation

Rectangular specimens with dimensions of 15 × 15 × 6 mm³ were machined from the tube wall. Each specimen was identified according to its heat-treatment condition, as summarized in Table 1. The experimental conditions included aging treatments performed at 850, 900, and 950 °C for 10, 100, and 1000 min, followed by either water quenching or furnace cooling.

2.3. Chemical Composition

The chemical characterization was performed by Optical Emission Spectroscopy (OES) using an Oxford Foundry Master Pro spectrometer, in accordance with ABNT NBR 16137:2016. The Pitting Resistance Equivalent Number (PREN) was calculated using a coefficient value of k = 20, as recommended by Nilsson (1992), Tan et al. (2009), and Weber and Uggowitzer (1998).

2.4. Differential Scanning Calorimetry (Dsc)

Differential Scanning Calorimetry (DSC) analyses were carried out using a Netzsch STA 449 F3 Jupiter thermal analyzer under an argon atmosphere. Samples were heated from 22 °C to 1200 °C at a rate of 10 °C/min. The DSC curves were used to identify the transformation and dissolution temperatures of intermetallic phases.

2.5. Thermodynamic Simulation

Thermodynamic simulations were performed using the FactSage 7.2 software with the FSstel steel alloy® database, based on the chemical composition determined by OES. The calculations predicted the equilibrium fractions of ferrite (α), austenite (γ), sigma (σ), chi (χ), secondary austenite (γ₂), and precipitates such as CrN, Cr₂N, M₇C₃, and M₂₃C₆ as a function of temperature.

2.6. Heat Treatments

Heat treatments were carried out in a high-temperature furnace (Fortelab MEZ 1700/4/E). Samples were first solution-annealed at 1125 °C for 5 min and quenched in water (condition TSL). Subsequent aging treatments were conducted at 850, 900, and 950 °C for 10 to 1000 min, followed by water quenching (TEA) or furnace cooling (TEF).

2.7. Microstructural Characterization

Specimens were ground, polished, and electrochemically etched according to ASTM E3-01 and ASTM E407-07. To distinguish the phases and precipitates, a 30% KOH electrolyte (2.5 V, 24 s) was used, followed by a 10% oxalic acid solution (6 V, 60 s) when required. Microstructural analyses were conducted using: Optical Microscopy (OM) - Olympus CX31 RTSF; Scanning Electron Microscopy with Energy Dispersive Spectroscopy (SEM/EDS) - TESCAN VEGA3, operating at 30 kV and 110 µA; X-ray Diffraction (XRD) - Bruker D8 Discover with Co-Kα radiation, operated at 40 mA and 35 kV, scanning from 2θ = 25° to 120°, with a step size of 0.01°. Phase volume fractions and grain sizes were quantified using ImageJ software (version 1.52n) following ASTM E562-19 and ASTM E1181-02 procedures.

2.8. Vickers Microhardness Test

The Vickers microhardness measurements were performed according to ASTM E384-17 using a Mitutoyo HM-12 microhardness tester. A load of 0.5 kgf and a dwell time of 20 s were applied, with 15 indentations per condition, discarding the highest and lowest readings. For phase-specific hardness measurements (ferrite and austenite + deleterious phases), a lower load of 0.05 kgf was employed.

3. Results and Discussion

3.1. Thermodynamic Simulation

The equilibrium phase diagram calculated (Figure 1) using FactSage 7.2 (database FSstel steel alloy®) indicated that the ferrite (α) and austenite (γ) phases coexist stably between 950 °C and 1100 °C, while the sigma (σ) phase becomes thermodynamically favored below 950 °C. Sigma nucleation occurs preferentially at α/γ interfaces, driven by the diffusion of Cr and Mo, consistent with recent findings by Pezzato and Calliari (2022) and Tütük et al. (2024).

3.2. Differential Scanning Calorimetry (Dsc)

The DSC (Figure 2) analysis revealed exothermic peaks near 850 °C associated with σ-phase formation and endothermic peaks between 950 °C and 1000 °C related to σ-phase dissolution. These transformations confirm the sensitivity of duplex stainless steels to thermal exposure and cooling rate, in agreement with Zhang et al. (2017).

3.3. Microstructural Evolution

OM observations (Figure 3) indicate a duplex microstructure with approximately balanced ferrite and austenite in the solution-annealed state; upon isothermal aging, σ-phase precipitates nucleate preferentially at α/γ interfaces and at ferrite grain boundaries, growing as elongated plates or blocky islands that consume the ferritic matrix. This nucleation behavior is governed by the local enrichment of Cr and Mo in ferrite and by the relative mobility of these species at elevated temperature, so that both the σ-phase volume fraction and precipitate size increase strongly with temperature and holding time (kinetically driven), consistent with experimental kinetic studies and thermodynamic predictions (Liu et al., 2023).
The morphology of σ (lamellar/needle-like vs. blocky) has direct consequences for properties: fine, dispersed σ may raise hardness via dispersion strengthening, whereas coarse or continuous σ at phase boundaries markedly reduces toughness and acts as a cathodic site that promotes localized corrosion adjacent to Cr-depleted zones. Thus, the observed pronounced σ precipitation after 1000 min at 950 °C explains the simultaneous increase in microhardness and the well-documented deterioration of pitting/crevice resistance when σ forms. These structure–property correlations are supported by both microstructural/property studies and micro-electrochemical analyses on UNS S32750 and related SDSS grades (Hosseini et al., 2018).

3.4. Sem/eds and X-Ray Diffraction Analysis

SEM/EDS mapping (Figure 4) confirmed Cr and Mo enrichment within σ precipitates and corresponding depletion in the adjacent ferritic matrix, explaining the local reduction in corrosion resistance (Tóth et al., 2024; Maurya et al., 2024). XRD diffractograms (Figure 5) exhibited σ-phase peaks near 44.5° and 47°, absent in the solution-treated samples, further confirming phase identification.

3.5. Phase Quantification

Image analysis showed a steady increase in σ-phase volume fraction (Table 2) with temperature and time, from approximately 3% (850 °C, 10 min) to > 15% (950 °C, 1000 min). Austenite grain coarsening and ferrite discontinuity were also observed, consistent with thermodynamic predictions.

3.6. Microhardness Behavior

The Vickers microhardness (Figure 6) increased proportionally to the σ-phase content, ranging from ~290 HV in the solution-annealed state to ~380 HV after aging at 950 °C/1000 min. This strengthening results from dispersion hardening by intermetallic precipitates, though at the expense of ductility and corrosion resistance, consistent with reports by Chen, Weng and Yang (2002) and Francis and Byrne (2021).

4. Conclusions

Thermodynamic modeling using FactSage 7.2 predicted σ-phase stability below 950 °C, in agreement with experimental evidence from DSC and microstructural analyses.
DSC analysis revealed distinct transformation peaks associated with σ-phase formation (~850 °C) and dissolution (~950-1000 °C), confirming the reversible nature of this phase under thermal cycling.
Microstructural and XRD observations demonstrated that σ-phase precipitates nucleate preferentially at α/γ interfaces and grow with temperature and exposure time, altering the ferrite/austenite balance.
EDS mapping confirmed local Cr and Mo enrichment in σ precipitates, explaining the expected deterioration of corrosion resistance.
Microhardness results indicated a direct correlation between σ-phase content and hardness increase, reflecting strengthening by intermetallic dispersion but concurrent loss of ductility.
The study establishes that precise control of heat input and aging parameters is critical to minimize deleterious σ-phase precipitation, ensuring the optimal combination of strength and corrosion resistance in super duplex stainless steels.

References

  1. Francis, R.; Byrne, G. Duplex Stainless Steels-Alloys for the 21st Century. Metals 2021, 11, 836. [Google Scholar] [CrossRef]
  2. Maurya, A.K.; Pandey, S.M.; Chhibber, R.; Fydrych, D.; Pandey, C. Corrosion performance of super duplex stainless steel and pipeline steel dissimilar welded joints: a comprehensive investigation for marine structures. Int. J. Adv. Manuf. Technol. 2024, 135, 1009–1033. [Google Scholar] [CrossRef]
  3. Pezzato, L.; Calliari, I. Advances in Duplex Stainless Steels. Materials 2022, 15, 7132. [Google Scholar] [CrossRef]
  4. Tütük, İ.; Ural, M.M.; Özer, G.; Kisasöz, A. Influence of Solution Treatment Process on the Properties of Duplex Stainless Steels: A Comparative Study on Microstructure and Corrosion Properties of UNS S32205 and UNS S32760. Metall. Mater. Trans. B 2024, 55, 2916–2921. [Google Scholar] [CrossRef]
  5. Tóth, T.; Hesse, A.-C.; Kárpáti, V.; Mertinger, V.; Dilger, K. Microstructural and mechanical properties of electron beam welded super duplex stainless steel. Weld. World 2024, 68, 1929–1940. [Google Scholar] [CrossRef]
  6. Nilsson, J.O. Super duplex stainless steels. Mater. Sci. Technol. 1992, 8, 685–700. [Google Scholar] [CrossRef]
  7. Tan, H.; Jiang, Y.; Deng, B.; Sun, T.; Xu, J.; Li, J. Effect of annealing temperature on the pitting corrosion resistance of super duplex stainless steel UNS S32750. Mater. Charact. 2009, 60, 1049–1054. [Google Scholar] [CrossRef]
  8. Weber, L.; Uggowitzer, P.J. Partitioning of chromium and molybdenum in super duplex stainless steels with respect to nitrogen and nickel content. Mater. Sci. Eng. A 1998, 242, 222–229. [Google Scholar] [CrossRef]
  9. Zhang, B.; Zhouhua, J.; Huabing, L.; Shucai, Z.; Hao, F.; Heng, L. Precipitation behavior and phase transformation of hyper duplex stainless steel UNS S32707 at nose temperature. Mater. Charact. 2017, 129, 31–39. [Google Scholar] [CrossRef]
  10. Chen, T.H.; Weng, K.L.; Yang, J.R. The effect of high-temperature exposure on the microstructural stability and toughness property in a 2205 duplex stainless steel. Mater. Sci. Eng. A 2002, 338, 259–270. [Google Scholar] [CrossRef]
  11. Liu, Z.; Xie, Y.; Chu, X.; Zhang, L.; Zhao, W.; Zhao, C.; He, H. Evolution of the sigma phase and its effect on the corrosion resistance of ASTM A890 3A duplex stainless steel. Mater. Today Commun. 2023, 36, 106926. [Google Scholar] [CrossRef]
  12. Hosseini, V.A.; Karlsson, L.; Wessman, S.; Fuertes, N. Effect of Sigma Phase Morphology on the Degradation of Properties in a Super Duplex Stainless Steel. Materials 2018, 11, 933. [Google Scholar] [CrossRef]
Figure 1. Calculated equilibrium phase fractions for UNS S32750 using FactSage. (Graph displaying phase fraction (%) vs. Temperature (°C) showing Ferrite, Austenite, Sigma, Alpha line, Chromium nitride, Chi, and Liquidus phases).
Figure 1. Calculated equilibrium phase fractions for UNS S32750 using FactSage. (Graph displaying phase fraction (%) vs. Temperature (°C) showing Ferrite, Austenite, Sigma, Alpha line, Chromium nitride, Chi, and Liquidus phases).
Preprints 243498 g001
Figure 2. Representative DSC curve showing σ-phase formation and dissolution peaks. (Thermal analysis curve plot: DSC (mW/mg) vs. Temperature (°C) with markers at 540 °C, 755 °C, 880 °C, 945 °C, 1 035 °C, and 1 100 °C).
Figure 2. Representative DSC curve showing σ-phase formation and dissolution peaks. (Thermal analysis curve plot: DSC (mW/mg) vs. Temperature (°C) with markers at 540 °C, 755 °C, 880 °C, 945 °C, 1 035 °C, and 1 100 °C).
Preprints 243498 g002
Figure 3. Comparative micrographs of solution-annealed and aged samples at 850 °C, 900 °C, and 950 °C. (Optical microscopy panels (a) to (d) for 850 °C, 900 °C, and 950 °C showing microstructure evolution, phase boundaries γ, δ, σ, χ, Cr2N, and 20 µm scale bars).
Figure 3. Comparative micrographs of solution-annealed and aged samples at 850 °C, 900 °C, and 950 °C. (Optical microscopy panels (a) to (d) for 850 °C, 900 °C, and 950 °C showing microstructure evolution, phase boundaries γ, δ, σ, χ, Cr2N, and 20 µm scale bars).
Preprints 243498 g003aPreprints 243498 g003b
Figure 4. SEM micrograph with EDS point analysis of the TEA 900/10 sample after electrolytic etching in 30% KOH solution. (SEM micrograph with chemical weight percentage tables (Wt%) for Austenite, Ferrite, Sigma, and Chromium nitride).
Figure 4. SEM micrograph with EDS point analysis of the TEA 900/10 sample after electrolytic etching in 30% KOH solution. (SEM micrograph with chemical weight percentage tables (Wt%) for Austenite, Ferrite, Sigma, and Chromium nitride).
Preprints 243498 g004
Figure 5. XRD patterns highlighting σ-phase peaks in aged samples. (Diffractogram series (a)-(d) showing Intensity vs. 2θ (degree) for TSL 1125/5, TEA/TEF 850, 900, 950 with phase peak labels γ, δ, σ).
Figure 5. XRD patterns highlighting σ-phase peaks in aged samples. (Diffractogram series (a)-(d) showing Intensity vs. 2θ (degree) for TSL 1125/5, TEA/TEF 850, 900, 950 with phase peak labels γ, δ, σ).
Preprints 243498 g005
Figure 6. Variation of microhardness with temperature and aging time. (Microhardness (HV) graph across conditions CR, TSL, 850 °C, 900 °C, 950 °C for TEA 10, TEA 100, TEA 1000, TEF 1000).
Figure 6. Variation of microhardness with temperature and aging time. (Microhardness (HV) graph across conditions CR, TSL, 850 °C, 900 °C, 950 °C for TEA 10, TEA 100, TEA 1000, TEF 1000).
Preprints 243498 g006
Table 1. Experimental conditions and sample identification codes.
Table 1. Experimental conditions and sample identification codes.
Conditionc Treatment / Parameters 10 min 100 min 1000 min (Water) 1000 min (Furnace)
As-received CR CR - 1 CR - 2 CR - 3 -
Solution Annealed 1125 °C / 5 min TSL - 1 TSL - 2 TSL - 3 -
Aged at 850 °C Water / Furnace TEA - 1 TEA - 4 TEA - 7 TEF - 10
TEA / TEF Series 2 TEA - 2 TEA - 5 TEA - 8 TEF - 11
TEA / TEF Series 3 TEA - 3 TEA - 6 TEA - 9 TEF - 12
Aged at 900 °C Water / Furnace TEA - 13 TEA - 16 TEA - 19 TEF - 22
TEA / TEF Series 2 TEA - 14 TEA - 17 TEA - 20 TEF - 23
TEA / TEF Series 3 TEA - 15 TEA - 18 TEA - 21 TEF - 24
Aged at 950 °C Water / Furnace TEA - 25 TEA - 28 TEA - 31 TEF - 34
TEA / TEF Series 2 TEA - 26 TEA - 29 TEA - 32 TEF - 35
TEA / TEF Series 3 TEA - 27 TEA - 30 TEA - 33 TEF - 36
Table 2. Measured phase volume fractions as a function of aging conditions.
Table 2. Measured phase volume fractions as a function of aging conditions.
Temperature (°C) Austenite (%wt) Ferrite (%wt) Sigma (%wt) Nitride (%wt)
850 54.0 32.5 8.5 3.9
900 51.5 46.0 - 2.5
950 51.0 49.0 - -
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.
Copyright: This open access article is published under a Creative Commons CC BY 4.0 license, which permit the free download, distribution, and reuse, provided that the author and preprint are cited in any reuse.