Preprint
Article

This version is not peer-reviewed.

Abrasive Wear of HH Heat-Resistant Stainless Steels Used in Pelletizing Furnace Grate Bars

Submitted:

06 November 2026

Posted:

09 November 2026

You are already at the latest version

Abstract
The abrasive wear of A297-HH heat-resistant stainless steel casting grate bars used to transport iron ore pellets in pelletizing furnaces was investigated. The grate bars operate under severe conditions, experiencing high temperatures and wear due to contact with the pellets. Microstructural analyses via metallography and Energy Dispersive Spectroscopy (EDS) identified chromium carbides (Cr23C6) and austenite, consistent with predictions from Thermo-Calc® software. Linear scratch tests were carried out using diamond and synthetic hematite Rockwell C indenters, applying progressive normal loads ranging from 0.2 to 10 N. Pin-on-disc wear tests were also performed to evaluate the tribological performance, using a synthetic hematite counter body to simulate real-world operating conditions. The predominant wear micromechanisms included micro-gouging and micro-cutting, with coefficients of friction ranging from 0.65 to 0.68 in the pin-on-disc tests. At 150°C in the pin-on-disc test, no mass loss was observed; instead, material transfer resulted in mass gain. The increase in microhardness in the wear tracks indicated surface work hardening. The results provide insights into wear mechanisms and material performance under different conditions, contributing to improved material selection and operational strategies.
Keywords: 
;  ;  ;  ;  

1. Introduction

Iron is one of the most abundant elements in the lithosphere and an essential mineral resource for the steel industry, being mined in large volumes. The central reserves are located in Brazil, Australia, China, India, Ukraine, Russia, the United States, Canada, and South Africa, and approximately 99% of global production is destined for the steel industry [1]. In Brazil, iron mining plays a crucial role in the economy, highlighted by its vast reserves and high-quality ore. In 2023, the Brazilian mining sector recorded revenues of US$33 billion and exported 359 million metric tons of iron ore, representing 15.5% of national exports [1].
Ore extraction and subsequent processing generate large amounts of fine particles, making their direct use in steelmaking processes unfeasible. To overcome this limitation, agglomeration processes such as sintering, pelletizing, and briquetting are used [2]. In pelletizing, ore pellets are transported through the furnace on grate cars and subjected to extreme thermal conditions. The grate bars, made of ASTM A297-HH stainless steel, undergo thermal cycles of 200 °C to 1100 °C in short intervals (30 min), in addition to creep, thermal fatigue, corrosion, and abrasive wear caused by contact with the pellets, especially during the discharge stage of the pellets into the furnace [2].
The annual consumption of these bars represents a high cost for pelletizing plants, not only due to material wear but also the costs associated with maintenance and production interruptions. This study investigates the abrasive wear of grate bars used in the Samarco Mineração pelletizing furnace through linear-sclerometry-scratch tests and pin-on-disc tests. Samples of A297-HH heat-resistant stainless steel in their as-cast condition were scratch tested with both diamond and synthetic hematite indenters, simulating an abrasive single-contact with the specimen's surface. In the pin-on-disc test, a spherical synthetic hematite counterbody was slid against discs made from the grate bars under different experimental conditions.
The applied normal load (4.5 N and 12 N), test temperature (23 °C and 150 °C), and disc surface roughness (0.05 µm and 0.5 µm) were varied to evaluate how these parameters affect the wear of A297-HH heat-resistant stainless steel. The mass loss and apparent friction coefficients were monitored throughout the tests to correlate the material's tribological behavior with its microstructure. Hematite was chosen because it is the major component of the ore pellets (approximately 62%), with 2.6% silica and 0.05% ferrite, reflecting real operating conditions [2].

2. Materials and Methods

1.1. Materials

The dimensions of the samples used in the tests were obtained from new grate bars manufactured in ASTM A297-HH heat-resistant stainless steel, as shown in Figure 1. This material was selected due to its high representativeness of the composition of iron ore pellets, which are composed of approximately 62% hematite, giving the material characteristics close to real operating conditions.
Hematite spheres were manufactured in accordance with ASTM G99-23 [3] to serve as counter bodies for the pin-on-disc tests. Similarly, hematite indenters were also manufactured in accordance with ASTM G171-03 [4] for the linear scratch test. The dimensions of the hematite sphere and of the indenters (scratch test standard) are depicted in Figure 2.

1.2. Methods

2.2.1. Sample Preparation

Polishing was performed in two stages using 3 μm and 1 μm diamond particle suspensions with a Struers TegraPol-25 automatic polisher. To evaluate the effect of roughness, three samples were tumbled on the Double Rotary Tumbler-10LT. Specimen cleaning included washing with soap, immersion in acetone, and ultrasonic cleaning for 10 minutes to remove impurities.
For the wear tests, the samples were washed with soap in running water, immersed in an acetone solution, and ultrasonically cleaned for 10 minutes. All handling was performed with gloves, avoiding contact with other objects.

2.2.2. Chemical, Metallurgical, and Mechanical Characterization

Microstructural characterization was performed using Optical Microscopy (OM) with a NIKON Eclipse MA200 microscope and Scanning Electron Microscopy (SEM) on a JEOL JSM-6010PLUS/LA instrument coupled with an Energy-Dispersive Spectroscopy (EDS) system for chemical analysis.
Thermodynamic simulations were also conducted using Thermocalc® software, using the TCS Steel and Fe-alloys Database (TCFE13) to predict the stability of the phases present in the steel after solidification. Furthermore, Vickers hardness (HV10) and microhardness (HV0.05) tests were performed on the samples before and after tribological testing using a Wolpert HT-1a and a SHIMADZU HMV-G 20ST, respectively.

2.2.3. Pin-On-Disc Wear Tests

The pin-on-disc tests were performed on a Phoenix Tribology Ltd. PLINT TE67 tribometer, following ASTM G99-23. The counter body (hematite sphere) slid against the steel discs under different experimental conditions, shown in Table 1.
The mass of the discs was measured before and after the tests, and the wear rate was calculated based on the mass loss and the volume of removed material. The wear tracks were characterized using SEM and EDS to identify transferred particles and the main degradation mechanisms.

2.2.4. Linear Scratch Tests

The scratch tests were performed on a CETR/Bruker APEX Universal Micro Tester Tribometer, following the ASTM G171-03 standard (2017), equipped with diamond and synthetic hematite Rockwell C indenters. Progressive normal loads, ranging from 0.2 to 10 N, were applied to the heat-resistant steel samples according to the parameters depicted in Table 2, and the apparent coefficients of friction were monitored along the scratch path. The surface preparation followed the same criteria established for the samples used in the pin-on-disc test. The wear paths were characterized by SEM and EDS analysis to identify the predominant wear micromechanisms.

3. Results and Discussions

3.1. Chemical, Metallurgical, and Mechanical Characterization

Table 3 presents the chemical composition of ASTM A297-HH heat-resistant steel, determined by optical emission spectrometry. It is a modified HH steel containing approximately 12% Mn. The Ni value was below the standard specified for conventional HH steel.
Optical Microscopy (OM) and Scanning Electron Microscopy (SEM) analyses revealed a microstructure composed of an as-cast matrix, with austenite dendrites and a eutectoid constituent (γ + M23C6) precipitated in the interdendritic regions, as shown in Figure 3. Dendrites formed during solidification under far-from-equilibrium conditions due to the heterogeneous temperature distribution during constitutional supercooling.
Table 4 presents a comparative analysis of the chemical composition measured by semi-quantitative EDS chemical analysis at the points indicated in Figure 4 and compares the EDS spectrometry results obtained with values reported in the literature for the γ and M23C6 phases, obtained in studies with standard ASTM A297-HH heat-resistant stainless steel (without Mn addition) [5,6,7].
Thus, points 1, 2, and 3 in Figure 4 show chemical compositions similar to the Cr23C6 carbide with additional manganese. Most probably, the manganese dissolved in the matrix is being detected due to X-ray emissions generated in the interaction volume, which is not strictly limited to the carbide but also encompasses the surrounding matrix. Points 4 and 5 show similarity to the reference composition for the austenitic matrix.
Thermodynamic simulation, using Thermocalc® (TCFE13), predicted the final microstructure of the grate bars, indicating the presence of austenite, MC, and Cr23C6 carbides, as shown in Figure 5. Unlike the results of Ding et al. (2016) [5], no residual ferrite was observed in the final microstructure, corroborating that, if adequate solubilization processes are employed, all delta ferrite is converted to austenite.
MC carbides could not be detected using the experimental techniques employed in this research. The absence of this constituent may be related to the characteristics of the material's solidification process. In contrast, the Thermocalc® thermodynamic analysis, which assumes equilibrium conditions, predicted MC carbide formation. However, this prediction reflects ideal behavior and may differ from the actual conditions of the analyzed material.
Evaluating the morphology, the quantitative analysis via EDS, and the results obtained from Thermocalc® software, a remarkable convergence between the data was observed, indicating consistency and robustness in the studies performed. The observed morphology is typical of Cr23C6 carbides, forming a eutectic microstructure. At the same time, the EDS analysis provided an elemental composition that corroborates the presence of these carbides, as predicted by Thermocalc thermodynamic models.
The hardness and microhardness measurement results for the grate bar and the synthetic hematite sphere are documented in Table 5.

3.2. Tribological Characterization

3.2.1. Pin-On-Disc Tests: Friction

The coefficients of friction (COFs) with a hematite sphere were determined for different conditions of temperature, normal load, and surface roughness. At 23 °C, with a polished surface (Ra ≈ 0.05 µm) and loads of 4.5 and 12 N, the coefficients of friction ranged from 0.65 to 0.68, as shown in Figure 6 and Figure 7.
For the sample subjected to a 12 N normal load, the average coefficient of friction was 0.65 ± 0.04 after the 100 s "running-in" period. In contrast, for the normal load of 4.5 N, the coefficient of friction stabilized around 400 seconds, with an average value of 0.68 ± 0.02.
Blau [8] emphasizes that friction force in a tribosystem rarely remains constant because of natural variations throughout the tests. Even in well-lubricated and designed systems, fluctuations in friction are inevitable, indicating the difficulty of eliminating the factors that influence their stability.
In the tests carried out at 150 °C, a temperature close to the actual working condition, the friction coefficient stabilized around 0.69 ± 0.04, as shown in Figure 8, possibly due to the formation of oxide debris at the tribological interface.
The range of variation of the coefficients of friction at 150°C, from 0.62 to 0.78, was greater than that observed for the tests carried out at room temperature.
When comparing the results of the wear tests performed with a 4.5 N load on samples subjected to 23°C and 150°C, the coefficients of friction presented almost similar average numerical values (0.68 and 0.72), although the variation of friction coefficients among different tests is much greater for the higher temperature test: the COF for Test 8 is 0.65, while the COF for Test 7 is 0.72. The COF for Test 9 is 0.78. These results suggest that the influence of temperature is not great enough to significantly impact the tribological behavior of the samples, although a greater dispersion of COF results may be observed. Based on the literature, 150°C was sufficient to soften the heat-resistant steel surface, favoring plastic deformation, adhesion mechanisms, and a slight increase in the coefficient of friction, as discussed by Soares et al. (2017) [9]. However, softening may have competed with the lubricating effect of the transferred hematite layer, influencing the material's tribological behavior.

3.2.2. Pin-On-Disc Test: Sliding Wear Rate

The wear rate was evaluated from mass loss and worn profiles using profilometry under different conditions. At 23 °C, Ra ≈ 0.05 µm and a load of 12 N, the average disc wear rate was (5.33 × 10-3) mm³/m. For the 4.5 N normal load, the coefficient of friction was (2.90 × 10-3) mm³/m. According to Archard, this phenomenon can be explained by the fact that an increase in normal load increases the real contact area. Thus, more contact points form between the asperities, increasing the probability of generating wear particles. Furthermore, increased load can intensify abrasion and adhesion mechanisms, contributing to a higher wear rate [10]. Table 6 shows the average wear rates for the different test conditions.
The wear-rate analysis shows that surface roughness does not significantly affect the wear of the steel studied. At 4.5 N, a marked difference was observed between tests at room temperature and 150°C. At this temperature, the disc gained mass due to hematite transfer from the sphere or oxidation of the worn surface.
Figure 9, obtained by SEM using secondary and backscattered electron detectors, shows the wear-track morphology, highlighting darker areas associated with hematite transfer from the sphere to the ASTM A297-HH heat-resistant stainless-steel disc. This image illustrates the significant accumulation of transferred material resulting from the sliding wear process. The observed considerable volume of material transferred suggests a predominantly adhesive wear mechanism on the disc surface.
Analysis of the average ball wear rate results under different experimental conditions reveals that the lowest value was obtained in the test conducted at 150°C, under an applied load of 4.5 N. This result is corroborated by the wear scar diameter after the test, as illustrated in Figure 10, which compares the wear scars under different temperature, roughness, and load conditions.
The smaller diameter of the sphere wear scar in the test carried out at 150°C, observed for the tests performed under the lowest load (4.5 N), indicates a reduction in the wear rate, possibly associated with the formation of a protective oxide layer on the surface of the heat-resistant steel. The increase in temperature favors oxidation, creating a barrier that reduces direct contact between the hematite sphere and the metal, minimizing abrasive wear.
Regarding the disc, it is likely that the particles detached from the hematite sphere adhered to the surface of the wear track, in conjunction with the oxidative processes that occur at high temperatures. This interaction makes it difficult to observe a decrease in the wear rate at 150 °C using the mass loss calculation. However, it is possible to note that, at elevated temperatures, the width of the wear track on the disc (Figure 11 d) was the smallest compared to the other test conditions.
The microhardness analysis of the wear track shown in Table 7 revealed a significant increase in surface hardness compared to the unworn material, indicating the occurrence of work hardening due to plastic deformation induced by tribological contact.
Work hardening influences the tribological behavior of metals, temporarily increasing surface hardness and wear resistance due to the accumulation of dislocations. However, continued sliding accumulates plastic deformation, generates local stresses, and causes depletion of deformation capacity, which favors the formation of microcracks and surface exfoliation, resulting in an increase in the microcracking wear rate in the long term [9,10,11].

3.2.3. Pin-On-Disc Test: Wear Track Morphology

In the tests at 150 °C, performed under a 4.5 N load, the wear track width was significantly smaller compared to samples evaluated at room temperature (Figure 12). This behavior may be related to the formation of an oxide layer or the transfer of material from the synthetic hematite sphere to the ASTM A297-HH heat-resistant stainless steel disc. The presence of debris adhered to the surface suggests that these materials may act as a solid lubricant, reducing direct contact between the surfaces and the severity of abrasive wear. This mechanism is consistent with studies indicating that oxides formed at high temperatures can act as protective barriers, and even as lubricants, reducing the wear rate [14,15]. Thus, the reduction in track width at 150 °C can be attributed to the formation of this protective layer.
Analysis of the wear track micrograph (Figure 13a) indicates the predominance of plastic mechanisms in the wear of the austenitic heat-resistant steel, evidenced by the presence of grooves and material transfer between the body and the counter body. Likely, the greater hardness of the hematite sphere compared to the steel disc favored initial groove formation and accelerated disc wear. Loose particles can adhere to the surfaces and act as microabrasive agents, being deformed and compacted by continuous sliding, resulting in the formation of transferred layers. The predominant presence of plastic wear is confirmed by the observation of scratches and grooves (Figure 13b), while brittle mechanisms, such as microcracks and material displacement, occur to a lesser extent.

3.2.4. Linear Sclerometry Test

In the scratching tests performed with diamond and hematite indenters, plastic behavior was observed in the formed tracks, despite the differences between the indenter types and the load variation (0.2 – 10 N). The tracks shown in Figure 16 presented distinct morphological characteristics, with the hematite indenter exhibiting an asymmetric cavity, suggesting that material may have adhered to the indenter due to the displacement observed along the track.
However, after a detailed inspection of the hematite indenter tip, which aimed to verify possible damage, the hypothesis of damage was ruled out. The groove and cutting mechanisms were identified in both tracks, as described by Hokkirigawa and Kato [16]. Measurements of the cross-sectional areas of the tracks, carried out with a three-dimensional analyzer, showed that the diamond indenter generated larger trenches than the hematite indenter, with a 16.6% difference in the trench cross-section at the central position of the scratch.
Linear scratch tests with diamond and hematite indenters showed that the apparent coefficient of friction stabilizes between 1 N and 3.5 N for both indenters. However, above 3.5 N (0.2 – 5 N progression) and 4.5 N (0.2 – 10 N progression), the coefficient of friction with the hematite indenter varies. In contrast, the value with the diamond indenter remains constant, as shown in Figure 17. In this Figure, one can see the graph of the apparent coefficient of friction evolution throughout the test. This variation can be attributed to the adhesion of material to the walls of the hematite indenter, altering the tribological contact conditions and favoring adhesive wear. The coefficient of friction for the diamond indenter stabilized around 0.17, a result in agreement with the data presented by Gong and Komvopoulos [17], who observed friction coefficients ranging from 0.16 to 0.17 for the heat-resistant steel surface. In contrast, for the hematite indenter, no comparisons were found in the literature.
Therefore, the results reached in this research indicate that cast austenitic heat-resistant steel has a typical microstructure, characterized by the presence of austenite dendrites and Cr23C6 carbides, as corroborated by analyses performed with Thermocalc®, scanning electron microscopy (SEM), and energy dispersive spectroscopy (EDS). Pin-on-disc tribological tests revealed coefficients of friction between 0.65 and 0.68 for normal loads of 4.5 and 12 N. At 150 °C, a slight increase in the coefficient of friction was observed, attributed to the formation of debris that alters the abrasion mechanism and the adhesion of the indenter material. The wear rate of the steel increased with the applied load. At the same time, the hematite sphere showed a lower wear rate under greater load, indicating a possible lubrication mechanism acting during the contact at high temperature.
The formation of a protective oxide layer at high temperatures and work hardening in the wear track highlight the complexity of wear mechanisms, which include plastic deformation and material transfer.
The morphological differences in the wear tracks between ambient and elevated temperatures highlight the importance of temperature in tribological interactions. The linear scratch test revealed that the material's scratch response exhibited plastic behavior, suggesting the adhesion of hard particles to the hematite indenter, evidenced by displacement marks in the track.

4. Conclusions

Taking into account the results and discussions previously presented regarding the tribology of the ASTM A297-HH heat-resistant stainless steel and hematite pair, it was concluded that:
• Cast ASTM A297-HH heat-resistant stainless steel exhibits a gross as cast microstructure composed of austenite dendrites and interdendritic eutectoid regions formed by (γ + Cr23C6).
• Tribological tests indicated coefficients of friction ranging from 0.65 to 0.68 for normal loads of 4.5 and 12 N at room temperature. The average coefficient of friction at 150°C was 0.69, indicating a negligible variation compared to tests performed under the same load at room temperature.
• Increasing the applied load (from 4.5 N to 12 N) resulted in a 90% increase in the wear rate of the ASTM A297-HH heat-resistant stainless steel, a phenomenon attributed to the increased contact pressure between the surfaces. Surface roughness, however, did not significantly influence the wear rate.
• In tests performed at 150 °C, under an applied load of 4.5 N, the disc showed mass gain, attributed to the transfer of material from the sphere to the disc. Furthermore, the width of the wear track was significantly smaller compared to the samples tested at room temperature.
• Analysis of the microhardness values along the wear track, performed under loads of 4.5 N and 12 N, both tested at room temperature (23 °C), revealed the occurrence of work hardening in the contact region between the hematite sphere and the disc.
• The wear mechanisms observed in the pin-disc test were governed by plastic deformation, as indicated by the presence of scratches and grooves on the surface.
• Significant differences in the morphology of the wear tracks were observed, especially regarding the presence of adhered material. The samples tested at 150°C showed a considerably larger volume of material adhered to the surface of the wear track.
• For the hematite sphere, the increased applied load resulted in a lower wear rate. The lowest wear rate was recorded at 150°C, associated with the formation of a protective oxide layer on the surface.
• In the linear scratch test, the scratch response indicated predominantly plastic behavior. Morphological analysis of the scratches revealed material adhesion to the indenter walls, influencing both the pit morphology and variations in the coefficient of friction between the hematite indenter and the stainless steel.

5. Acknowledgments

The authors would like to thank Samarco Mineração S.A. for funding the research project related to this work and for the SEM images.

References

  1. Pereira, S. de A. C. The iron ore market (Specialization thesis in Mineral Resources Engineering). Federal University of Minas Gerais, Minas Gerais, Brazil, 2012.
  2. Chagas, M. Modeling and operational control of the pelletizing process through the method of artificial neural networks (Master’s thesis). Federal Institute of Espírito Santo, Vitória, Brazil.
  3. ASTM G99-23, Standard Test Method for Wear Testing with a Pin-On-Disk Apparatus, 2023.
  4. ASTM G171-03, Standard Test Method for Scratch Hardness of Materials Using a Diamond Stylus, West Conshohocken, PA, vol. 2017, 2017.
  5. Ding, Xf., Liu, Df., Guo, Pl. et al. Solidification microstructure formation in HK40 and HH40 alloys. Int J Miner Metall Mater 23, 442–448, 2016.
  6. Bagheri, M., Pourdehsheykhi, H., Kermani, S. M., & Pourmahyabadi, A. Damage characterization of heat resistant stainless steel grate plates in an iron ore pelletizing plant. Engineering Failure Analysis, 110, 104414, 2020.
  7. Sorensen, C. D., & Nelson, T. W. Sigma phase formation in friction stirring of iron-nickel-chromium alloys. In Proceedings of the Trends in Welding Research, Proceedings of the Seventh International Conference, 2005.
  8. Blau, P. J. Friction science and technology: from concepts to applications. CRC press, 2008.
  9. Soares, G. C., Rodrigues, M. C. M., & Santos, L. D. A. Influence of temperature on mechanical properties, fracture morphology and strain hardening behavior of a 304 stainless steel. Materials Research, 20(Suppl 2), 141-151, 2017.
  10. Zum Gahr, K. H. Microstructure and wear of materials (Vol. 10). Elsevier, 1987.
  11. Zhang, K., Liu, D., & Zhao, X. The Role of Ductility and Work Hardening in Sliding Wear of an Al–Zn–Mg–Cu Alloy. Transactions of the Indian Institute of Metals, 75(3), 749-755, 2022.
  12. Sun, G., Huang, J., Peng, J., & Wu, W. Effect of strain hardening on wear and corrosion resistance of 316L Austenitic stainless steel. Journal of Materials Engineering and Performance, 33(16), 8108-8121, 2024.
  13. Sheng, S., Zhou, H., Wang, X., Qiao, Y., Yuan, H., Chen, J., ... & Zou, J. Friction and Wear Behaviors of Fe-19Cr-15Mn-0.66 N Steel at High Temperature. Coatings, 11, 1285. Corrosion and Degradation of Materials, 321, 2021.
  14. Harfouche, M. M., Alidokht, S. A., Grandy, L., Aghasibeig, M., Mauzeroll, J., & Chromik, R. R. Microstructural, Micromechanical, Wear, and Corrosion Properties of Cold Spray and Laser-Assisted Cold Spray CrMnCoFeNi Cantor HEA Coatings. Journal of Thermal Spray Technology, 34(2), 550-569, 2025.
  15. Zhang, H., Wang, L., Hu, J., Wang, G., & Xu, W. Optimum wear resistance achieved by balancing bulk hardness and work-hardening: a case study in austenitic stainless steels. Tribology Letters, 71(1), 7, 2023.
  16. Hokkirigawa, K., & Kato, K. An experimental and theoretical investigation of ploughing, cutting and wedge formation during abrasive wear. Tribology international, 21(1), 51-57, 1988.
  17. Gong, Z. Q., & Komvopoulos, K. Mechanical and thermomechanical elastic-plastic contact analysis of layered media with patterned surfaces. Journal of tribology, 126(1), 9-17, 2004.
Figure 1. Locations from which specimens were extracted for testing.
Figure 1. Locations from which specimens were extracted for testing.
Preprints 242856 g001
Figure 2. Hematite sphere, hematite indenter, and diamond indenter.
Figure 2. Hematite sphere, hematite indenter, and diamond indenter.
Preprints 242856 g002
Figure 3. Microstructure of the grate bar. (a) Etching with 50% hydrochloric acid (HCl) solution + 35% PA alcohol + 15% nitric acid (HNO3). OM, magnification: 50x; (b) OM, magnification: 1,000X.
Figure 3. Microstructure of the grate bar. (a) Etching with 50% hydrochloric acid (HCl) solution + 35% PA alcohol + 15% nitric acid (HNO3). OM, magnification: 50x; (b) OM, magnification: 1,000X.
Preprints 242856 g003
Figure 4. Energy-dispersive spectrometry (EDS) of ASTM A297 HH – high-Mn steel. SEM, magnification: 3,300x.
Figure 4. Energy-dispersive spectrometry (EDS) of ASTM A297 HH – high-Mn steel. SEM, magnification: 3,300x.
Preprints 242856 g004
Figure 5. Scheil modeling in modified ASTM A297-HH heat-resistant stainless steel.
Figure 5. Scheil modeling in modified ASTM A297-HH heat-resistant stainless steel.
Preprints 242856 g005
Figure 6. Coefficient of friction as a function of total test time at room temperature under a 4.5 N load for the austenitic heat-resistant steel/hematite tribological pair. The gray dots represent the unprocessed data, while the solid lines correspond to the data processed with a 90-point moving average filter for the three replicates tested.
Figure 6. Coefficient of friction as a function of total test time at room temperature under a 4.5 N load for the austenitic heat-resistant steel/hematite tribological pair. The gray dots represent the unprocessed data, while the solid lines correspond to the data processed with a 90-point moving average filter for the three replicates tested.
Preprints 242856 g006
Figure 7. Coefficient of friction as a function of total test time at room temperature under a 12 N load for the austenitic stainless steel and hematite tribological pair. The gray dots represent the unprocessed data, while the solid lines correspond to the data processed with a 90-point moving average filter, for the three replicates tested.
Figure 7. Coefficient of friction as a function of total test time at room temperature under a 12 N load for the austenitic stainless steel and hematite tribological pair. The gray dots represent the unprocessed data, while the solid lines correspond to the data processed with a 90-point moving average filter, for the three replicates tested.
Preprints 242856 g007
Figure 8. Coefficient of friction as a function of total test time at 150 °C under a 4.5 N load for the austenitic heat-resistant steel/hematite tribological pair. The gray points represent the unprocessed data, while the solid lines correspond to the data processed with a 90-point moving average filter, for the three replicates tested.
Figure 8. Coefficient of friction as a function of total test time at 150 °C under a 4.5 N load for the austenitic heat-resistant steel/hematite tribological pair. The gray points represent the unprocessed data, while the solid lines correspond to the data processed with a 90-point moving average filter, for the three replicates tested.
Preprints 242856 g008
Figure 9. Scanning electron microscopy (SEM) images of the tribological pair of hematite sphere and austenitic stainless steel, using secondary electron (SEI) and backscattered electron (BES) detection modes, evidencing the presence of iron oxide particles on the surface of the disc, suggesting an adhesive wear mechanism, in which part of the sphere material adheres to the surface of the disc during the sliding process.
Figure 9. Scanning electron microscopy (SEM) images of the tribological pair of hematite sphere and austenitic stainless steel, using secondary electron (SEI) and backscattered electron (BES) detection modes, evidencing the presence of iron oxide particles on the surface of the disc, suggesting an adhesive wear mechanism, in which part of the sphere material adheres to the surface of the disc during the sliding process.
Preprints 242856 g009
Figure 10. Wear scar diameters on the hematite sphere after wear tests with varying load, surface roughness, and temperature.
Figure 10. Wear scar diameters on the hematite sphere after wear tests with varying load, surface roughness, and temperature.
Preprints 242856 g010
Figure 11. Dimension of the wear tracks for the tested samples according to variations in load, temperature, and surface roughness.
Figure 11. Dimension of the wear tracks for the tested samples according to variations in load, temperature, and surface roughness.
Preprints 242856 g011
Figure 12. Samples ASTM A297-HH heat-resistant stainless-steel disc after pin-on-disc test.
Figure 12. Samples ASTM A297-HH heat-resistant stainless-steel disc after pin-on-disc test.
Preprints 242856 g012
Figure 13. Wear track of the ASTM A297-HH heat-resistant stainless-steel disc after sliding against a hematite sphere. (a) under load 4.5 N; (b) under load 12 N.
Figure 13. Wear track of the ASTM A297-HH heat-resistant stainless-steel disc after sliding against a hematite sphere. (a) under load 4.5 N; (b) under load 12 N.
Preprints 242856 g013
Figure 16. Scratch ditches under a load of approximately 8 N. (a) With diamond indenter; (b) With hematite indenter.
Figure 16. Scratch ditches under a load of approximately 8 N. (a) With diamond indenter; (b) With hematite indenter.
Preprints 242856 g014
Figure 17. Coefficient of friction as a function of normal load during the scratch test. (a) 0.2 – 5 N; (b) 0.2 – 10 N.
Figure 17. Coefficient of friction as a function of normal load during the scratch test. (a) 0.2 – 5 N; (b) 0.2 – 10 N.
Preprints 242856 g015
Table 1. Pin-on-disc test parameters.
Table 1. Pin-on-disc test parameters.
Test Parameters
Normal loads [N] 4.5 12
Temperatures [°C] 23 150
Sliding speed [RPM] 210
Test time [s] 1,800
Table 2. Linear scratch test parameters for both indenter types.
Table 2. Linear scratch test parameters for both indenter types.
Test Parameters
Indenter Type Diamond Hematite
Preload [N] 0.2 0.2
Preload duration [s] 2.0 2.0
Load [N] 0.2 – 5.0
0.2 – 10.0
0.2 – 5.0
0.2 – 10.0
Speed [mm/s] 0.1 0.1
Scratch length [mm] 5.0 5.0
Number of scratch replicas 3 3
Table 3. Chemical composition of the modified ASTM A297-HH heat-resistant stainless steel.
Table 3. Chemical composition of the modified ASTM A297-HH heat-resistant stainless steel.
Cr [wt.%] Ni [wt.%] Mo [wt.%] Si [wt.%] Mn [wt.%] P [wt.%] S [wt.%] C [wt.%]
ASTM A297-HH heat-resistant stainless steel 22.90 8.36 0.39 1.43 11.98 0.04 0.02 0.30
Table 4. Chemical composition measured by EDS.
Table 4. Chemical composition measured by EDS.
Cr [wt.%] Ni [wt.%] Si [wt.%] Mn [wt.%] Fe [wt.%]
Spot 1 63.4 3.3 - 9.5 23.7
Spot 2 64.1 3.4 - 9.5 22.9
Spot 3 65.0 2.9 0.3 9.10 22.6
Spot 4 25.7 11.6 0.9 12.7 49.0
Spot 5 25.0 11.5 0.8 12.3 50.3
M 23 C 6 reference [3,4,5] 60.3-72.3 2.1-2.3 - - 25.3-27.7
γ reference [3,4,5] 15.5-22.2 13.8-16.3 - - 63.9-68.3
Table 5. Hardness and microhardness test results.
Table 5. Hardness and microhardness test results.
Material Microhardness (HV0.05) Hardness (HV10)
ASTM A297-HH heat-resistant stainless steel - 196 ± 4
Hematite sphere 877 ± 12 -
Table 6. Average wear rate ‘Q’ [mm3/m] for the different pin-on-disc test conditions.
Table 6. Average wear rate ‘Q’ [mm3/m] for the different pin-on-disc test conditions.
Temperature [°C] Ra [µm] Load [N] ‘Q’ Disc [mm3/m] ‘Q’ Pin [mm3/m]
23 0.5 12 5.53 x 10-3 7.14 x 10-3
23 0.05 12 5.33 x 10-3 6.09 x 10-3
23 0.05 4.5 2.90 x 10-3 7.55 x 10-3
150 0.05 4.5 2.57 x 10-4 7.97 x 10-4
Table 7. Vickers microhardness of the wear track after the pin-on-disc test with 4.5 N and 12 N.
Table 7. Vickers microhardness of the wear track after the pin-on-disc test with 4.5 N and 12 N.
Microhardness [HV0.05] Error
[%]
Before pin-on-disc testing 196 ± 4
On the wear scar after 12.0 N testing 493 ± 5
On the wear scar after 4.5 N testing 430 ± 5
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.
Copyright: This open access article is published under a Creative Commons CC BY 4.0 license, which permit the free download, distribution, and reuse, provided that the author and preprint are cited in any reuse.