Submitted:
30 October 2026
Posted:
02 November 2026
You are already at the latest version
Abstract
Electrocatalysts for sustainable energy conversion must be active, selective and durable while making efficient use of scarce metals. This work reviews palladium (Pd)- and rhodium (Rh)-based nanomaterials, compares their design principles with those of hydrogenases and formate dehydrogenases, and discusses electrodeposition from choline chloride–urea deep eutectic solvents (DESs). As a case study, Pd, Rh and Pd–Rh deposits were prepared on glassy carbon and characterized by scanning electron microscopy, energy-dispersive X-ray spectroscopy, cyclic voltammetry, X-ray diffraction and X-ray photoelectron spectroscopy. These techniques describe morphology, elemental distribution, deposition behaviour, crystal structure and surface chemical state, but they do not by themselves establish catalytic activity, selectivity, durability or an environmental advantage. Recent studies on Pd electrocatalysts and on electrochemistry in DESs are used to place the results in context. The discussion also relates catalyst development to green chemistry, the circular economy and the United Nations 2030 Agenda. We argue that sustainability claims need quantitative data on metal loading, activity, stability, metal leaching, solvent recovery, energy demand, waste and, where possible, life-cycle impacts. Pd/Rh nanomaterials prepared in DESs are therefore presented as a promising research direction whose practical value has yet to be demonstrated.

Keywords:
electrocatalysis
; palladium
; rhodium
; nanomaterials
; deep eutectic solvents
; hydrogenase
; formate dehydrogenase
; electrodeposition
; green chemistry
; circular economy
; sustainability
1. Introduction
Solar and wind power are central to a lower-carbon energy system, but the transition also depends on technologies to store energy, convert it into other forms and produce chemicals with a smaller environmental footprint. Electrochemistry contributes in several ways: fuel cells convert chemical energy into electricity, and electrolysers use electricity to drive chemical reactions. The electrochemical conversion of captured carbon dioxide (CO₂) into useful products with low-carbon electricity is also being actively investigated [1,2].
Many of these reactions are slow under practical conditions, require large overpotentials or produce unwanted by-products. A catalyst lowers these barriers by providing surface sites at which reactants adsorb and exchange electrons with the electrode. Ideally, it also improves selectivity and stability and reduces the energy input [1,3].
For this reason, the electrode surface, where the solid, the electrolyte and the reacting molecules meet, largely determines the outcome of an electrocatalytic reaction, and small changes at this interface can alter both the rate and the product distribution.
Current approaches to electrocatalyst design aim to relate atomic-scale structure to reaction pathways and long-term stability; a high surface area alone is not considered sufficient. In formic acid oxidation, for example, the main challenge remains the balance between activity, pathway selectivity and resistance to deactivation. Recent Pd-based catalysts use alloying, confinement and control of local atomic order to tune the binding of intermediates and improve durability, although a fair comparison between them requires consistent metal loadings, electrochemical protocols and stability criteria [4,5,6,7].
2. Why Make A Catalyst Nanoscale?
A nanometre is one billionth of a metre. When a metal is dispersed as very small particles, a larger fraction of its atoms lies at the surface, where most catalytic reactions take place, so each gram of metal can be used more effectively. The actual gain depends on how many of these surface atoms are accessible and active, and not only on the nominal particle size [1,3].
Decreasing the particle size also has drawbacks. Nanoparticles may agglomerate, dissolve or restructure during operation, and their behaviour depends on shape, crystal structure, surface chemistry and the surrounding electrolyte. Samples with similar particle sizes can therefore perform quite differently.
Combining two metals offers a further means of tuning the surface. In materials containing palladium (Pd) and rhodium (Rh), the arrangement and relative amounts of the two elements may modify the adsorption of reactants and intermediates and, consequently, the reaction pathway. Such effects have to be verified experimentally, which requires linking preparation conditions, structure and electrochemical performance [1,3].
3. Palladium and Rhodium: Useful Materials, Not Magic Ingredients
Palladium is studied as a catalyst for the electro-oxidation of small organic molecules such as methanol and formic acid, which are of interest for direct liquid fuel cells, devices that convert the chemical energy of a liquid fuel directly into electricity. Pd-based materials are also investigated for some CO₂-reduction pathways, although the products and efficiencies depend strongly on the catalyst and the operating conditions [8,9,10,11]. Recent work shows that the activity and durability of Pd can be modified by alloying, confinement, surface strain and control of local atomic order [4,5,6,7]. These studies provide useful design strategies, but they concern other Pd-containing systems; the catalytic performance of the Pd–Rh deposits described here was not measured and cannot be inferred from them.
Rhodium has distinct catalytic properties of its own, and its combination with Pd raises the question of whether composition or surface arrangement can be used to tune the electrode response. The answer depends on how the material forms, how the two elements are distributed and how the surface evolves under electrochemical operation.
Because both metals are expensive, they must be used efficiently. Dispersing small amounts of metal on a conductive support can increase the fraction of accessible atoms, and alloying may change catalytic behaviour. Nevertheless, detecting both metals by elemental analysis does not demonstrate that a homogeneous alloy has formed, nor that the material is more active than a monometallic control.
4. Lessons From Nature’s Catalysts
Long before nanocatalysts were developed, living organisms evolved enzymes that catalyse some of the same reactions. Hydrogenases, present in many bacteria, archaea and algae, interconvert protons and hydrogen at active sites containing iron alone or iron and nickel. Formate dehydrogenases, some of which contain molybdenum or tungsten, interconvert formate and carbon dioxide; both reactions are relevant to formic acid oxidation and CO₂ conversion [9,10,12,13]. A recent review of direct enzyme electrochemistry describes how electrode wiring, protein orientation and electron-transfer pathways determine catalytic directionality, reversibility and oxygen tolerance [14].
When some of these enzymes are adsorbed on an electrode (protein film electrochemistry), they catalyse their reactions in both directions at very small overpotentials. This efficiency arises from the highly organized environment of the metal site: the protein positions the substrate, transfers protons and electrons along defined pathways and stabilizes intermediates. In effect, the protein provides the kind of surface control that materials scientists seek by adjusting particle size, composition and support [13,15].
Enzymes cannot simply replace metal catalysts. Many are sensitive to oxygen, difficult to produce on a large scale and less durable than inorganic materials under device conditions. They are nevertheless useful benchmarks of efficiency and selectivity, and they show that the environment around the active site can be as important as the metal itself. Bioinspired and hybrid systems, which combine enzymes or enzyme-like sites with conductive materials, are being developed at this interface between biochemistry and electrocatalysis [12,15].
5. Preparing Modified Electrodes with A Deep Eutectic Solvent
Electrodeposition is a convenient way of preparing and studying metal surfaces: dissolved metal species are reduced by an applied potential to form a deposit on a conductive substrate. Varying the solution composition and the deposition conditions makes it possible to examine how metal nuclei form and grow.
Deep eutectic solvents (DESs) are mixtures with a melting point lower than that of their individual components; a widely studied example is the mixture of choline chloride and urea. Depending on their composition, DESs can serve as alternative media for dissolving metal salts and for electrochemical synthesis [16,17]. The structure of the electrode–DES interface affects metal nucleation [18], and nucleation and growth in DESs can differ considerably from those in aqueous solutions [19]. Pd nanoparticles electrodeposited from a DES have been evaluated for formic acid oxidation [20], and Pd–Ag alloy nanoparticles have been deposited from ethaline on bare and polymer-modified glassy carbon [21].
Similar liquids may also occur in living cells. Choline chloride, the most common DES component, is a salt of choline, an essential nutrient, and mixtures of sugars, organic acids, amino acids and choline have been proposed to form natural deep eutectic solvents (NADESs) in plants. These liquids may help cells to survive drought or freezing and to dissolve poorly water-soluble metabolites. The same class of liquids is therefore of interest both in cell physiology and in electrode preparation [22,23].
DESs should not be regarded as “green” by default. Their environmental profile depends on the components and their sourcing, the energy needed for preparation, recovery and reuse, toxicity and end-of-life treatment. A 2025 review noted that the carbon footprint and environmental fate of many DES formulations are still poorly quantified and proposed life-cycle assessment as the appropriate framework [24]. DESs are better described as alternative preparation media whose advantages must be evaluated case by case.
A recent review of electrocatalysis in DESs highlights their influence on precursor solubility, nucleation, morphology and the electrode–electrolyte interface, and points out open questions regarding mass transport, solvent composition and scale-up [25]. In the choline chloride–urea system used here, temperature and viscosity therefore affect the deposition mechanism directly. Any sustainability claim would also require data on solvent recovery and reuse, energy consumption and waste generation.
6. How Do We Know What We Have Made?
6.1. Experimental Details of the Illustrative Example
The electrodes shown in Figure 1, Figure 2, Figure 3, Figure 4, Figure 5 and Figure 6 were prepared and characterized as part of the doctoral research of V. A. Medina Rojano. The deep eutectic solvent (DES) was prepared by mixing choline chloride (ChCl, ≥98%, Sigma-Aldrich, St. Louis, MO, USA) and urea (U, ≥98%, Sigma-Aldrich) in a 1:2 molar ratio, corresponding to the eutectic composition reported by Abbott et al. [16]. The mixture was heated at 70 °C under continuous magnetic stirring for 24 h until a clear, homogeneous liquid phase was obtained. Metal precursor solutions were prepared by dissolving palladium(II) chloride (PdCl₂, ≥99.9%, Sigma-Aldrich) and rhodium(III) chloride (RhCl₃, ≥99.9%, Sigma-Aldrich) in the DES to give 50 mM PdCl₂ and 25 mM RhCl₃ for the monometallic solutions and 25 mM of each salt for the bimetallic solution.
Before each experiment, the glassy-carbon electrode (GCE; 5 mm diameter, geometric area 0.196 cm²) was polished successively with 1, 0.3 and 0.05 µm alumina on a MicroCloth polishing pad (Buehler, Lake Bluff, IL, USA), cleaned in an ultrasonic bath of deionized water (18.2 MΩ cm) for 15 min and dried. Cyclic voltammograms were recorded on the GCE in the DES containing 50 mM PdCl₂, 25 mM RhCl₃, or 25 mM PdCl₂ + 25 mM RhCl₃, at scan rates of 10–50 mV s⁻¹; the potential was scanned from 0 V first to +0.6 V (+1.2 V for the mixed solution), then to −1.0 V and back to 0 V. An Ag quasi-reference electrode (QRE) and a platinum-wire counter electrode were used; the temperature was 70 °C, at which the DES has a lower viscosity and a higher conductivity than at room temperature, as in previous electrodeposition studies in the same solvent [26]. Measurements were performed with an Autolab PGSTAT30 potentiostat/galvanostat (Metrohm Autolab, Utrecht, The Netherlands) controlled by NOVA 2.1 software. Pd, Rh, and Pd–Rh deposits were obtained by potentiostatic electrodeposition for 60 s at −0.20, −0.22, −0.24, −0.26, −0.28 and −0.30 V; for the Rh(III) solution, current–time transients were additionally recorded between −0.98 and −1.30 V. The transients and the parameters derived from them are given in Figure S1–S3 and Table S1 and Table S2. The deposits characterized by SEM, EDX, X-ray diffraction and XPS were prepared at −0.28 V. Surface morphology was examined by scanning electron microscopy (SEM), and elemental composition/distribution by energy-dispersive X-ray spectroscopy (EDX). SEM and EDX measurements were performed at the Escuela Superior de Ingeniería Química e Industrias Extractivas (ESIQIE), Instituto Politécnico Nacional, using a JEOL JSM-6701F field-emission scanning electron microscope (JEOL Ltd., Akishima, Tokyo, Japan) equipped with an Oxford Instruments energy-dispersive X-ray detector (Oxford Instruments, High Wycombe, UK). Images were acquired at an accelerating voltage of 10 kV and working distances of 6.9–8.3 mm, and EDX spectra were collected at multiple points across each sample.
X-ray photoelectron spectroscopy (XPS) was measured on Pd and Pd–Rh deposits prepared on glassy carbon as described above (−0.28 V, 60 s, 70 °C; 50 mM PdCl₂ or 25 mM PdCl₂ + 25 mM RhCl₃). Spectra were recorded on a K-Alpha spectrometer (Thermo Fisher Scientific, East Grinstead, UK) at the Instituto Mexicano del Petróleo (IMP; base pressure ~2 × 10⁻⁹ mbar) with a monochromatic Al Kα source (hν = 1486.6 eV). Survey spectra were acquired with a step size of 1 eV, and high-resolution Pd 3d, Rh 3d, C 1s and O 1s spectra with a step size of 0.1 eV. Binding energies were referenced to adventitious C 1s at 284.8 eV. Spectra were fitted with Gaussian–Lorentzian components after Shirley background subtraction using Thermo Avantage software, and surface compositions were calculated from the survey spectra.
The X-ray diffraction (XRD) pattern of the Pd–Rh deposit, prepared under the same conditions and fixed to the sample holder with double-sided conductive carbon tape, was recorded on a Bruker D8 Advance diffractometer (Bruker AXS, Karlsruhe, Germany) with Cu Kα radiation (λ = 1.5406 Å; 40 kV, 40 mA) over 2θ = 20–100° with a step size of 0.01°; the 20–80° region, which contains all the observed reflections, is shown in Figure 5. Reflections were indexed against the reference patterns of Pd (PDF 46-1043) and Rh (PDF 05-0685). The lattice parameter was calculated from the (111), (200) and (220) reflections, the Rh fraction was estimated with Vegard’s law using a(Pd) = 3.890 Å and a(Rh) = 3.804 Å, and the crystallite size was estimated with the Scherrer equation (K = 0.9) from the full width at half maximum of the (111) reflection fitted with a pseudo-Voigt function.
6.2. Microscopy, Elemental Analysis and Electrochemistry
No single technique provides a complete description of an electrocatalyst. Scanning electron microscopy (SEM) images show the surface morphology and allow coverage, particle features and aggregation to be compared, whereas energy-dispersive X-ray spectroscopy (EDX) identifies the elements present in the analysed region, and elemental maps show how they are distributed.
Both techniques have limitations. EDX results depend on the substrate, the sampling volume and the measurement conditions, and EDX alone cannot determine oxidation states or prove that two metals form a homogeneous alloy. Other techniques are required when the crystal structure, chemical state or atomic-scale mixing is central to the interpretation.
Figure 1, Figure 2 and Figure 3 show the results for Pd, Rh and Pd–Rh deposits obtained on glassy carbon from choline chloride–urea DES. Pd forms isolated, quasi-spherical particles, Rh forms much smaller particles grouped in agglomerates, and co-deposition produces a dense layer of larger, faceted particles, which indicates that the presence of both metals changes the nucleation and growth of the deposit. EDX confirms the presence of Pd and Rh and shows their distribution; however, because the Pd L and Rh L lines partially overlap, the maps alone cannot establish whether an alloy has formed.
Electrochemical methods probe the response of an electrode to an applied potential. In cyclic voltammetry, the potential is swept over a selected range while the current is recorded, which reveals surface and redox processes under the chosen conditions. In chronoamperometry, the potential is held constant and the current is followed over time.
Cyclic voltammetry can also be used before deposition, to understand how metal ions are reduced in the solvent. Figure 4 shows voltammograms recorded on glassy carbon in choline chloride–urea containing Pd(II), Rh(III) or both, with potentials referred to an Ag quasi-reference electrode. On the cathodic scan, Pd(II) shows a small reduction wave from about +0.1 V and a broad peak at about −0.80 V, whereas the reduction of Rh(III) starts only at about −0.3 to −0.5 V, depending on the scan rate, with a peak at about −0.82 V, consistent with the easier reduction of the Pd species. On the anodic scan, Pd shows a sharp stripping (re-oxidation) peak near +0.35 V (1.3 mA cm⁻² at 50 mV s⁻¹), whereas Rh shows only a weak anodic feature near −0.2 V (0.27 mA cm⁻²), consistent with its limited dissolution in this medium. In the mixed solution, reduction starts at about −0.15 V, a well-defined cathodic peak appears at −0.30 to −0.38 V and a single stripping peak appears near +0.6 V, at a potential different from those of either metal alone. This behaviour suggests that the two metals interact during deposition, possibly forming a mixed or alloyed phase, a possibility examined by X-ray diffraction (XRD) and X-ray photoelectron spectroscopy (XPS) in Section 6.3. Only the mixed solution shows a nucleation loop, in which the anodic scan crosses the cathodic scan, as is characteristic of metal deposition on a foreign substrate [26]. The crossover at about 0.00–0.04 V approximates the equilibrium potential of the co-deposition process, so the deposition potentials used here (−0.20 to −0.30 V) correspond to cathodic overpotentials of roughly 0.2–0.3 V. The currents in the mixed solution are also roughly an order of magnitude higher than those for Pd(II) alone (anodic peaks of about 12.8 and 1.3 mA cm⁻², respectively, at 50 mV s⁻¹), despite the lower concentration of each salt, a difference that merits further study. In this work, these measurements were used to choose the potential window for deposition.
The current–time transients recorded during deposition (Figure S1) complement the voltammetric data. For Pd and Pd–Rh, the transients show the current rise characteristic of three-dimensional nucleation and growth throughout the potential range used (−0.20 to −0.30 V). The Rh(III) solution, in contrast, gives an appreciable deposition current only at about −1.0 V and more negative potentials (Figure S1b and Figure S2). The Rh deposit prepared at −0.28 V should therefore be interpreted with caution, because the very small current at this potential indicates that only a small amount of Rh-containing material was formed. The higher current in the mixed solution suggests that Pd facilitates the incorporation of Rh during co-deposition, although transients alone cannot prove alloy formation. Between −0.20 and −0.30 V, the time of the current maximum decreases from 0.55 to 0.10 s for Pd and from 4.39 to 0.61 s for Pd–Rh, while the charge passed in 5 s increases from 0.33 to 0.41 mC and from 0.65 to 2.41 mC, respectively (Table S1 and Table S2, Figure S3); nucleation is thus considerably slower for the co-deposit than for Pd. In this chloride-rich solvent, the metal ions are expected to be present as chloro-complexes whose stability affects their reduction, as reported for Cu(I) in the same medium [27]. Together with the XPS composition (Section 6.3), these results indicate that Rh is incorporated into the co-deposit at potentials about 0.7 V less negative than those required for significant deposition from the Rh(III) solution alone (Figure S3).
6.3. Crystal Structure and Surface Chemical State
Figure 5 shows the XRD pattern of the Pd–Rh deposit. A single set of face-centred cubic (fcc) reflections is observed, with the (111), (200) and (220) peaks at 40.55°, 46.94° and 68.87°, respectively, each located between the corresponding positions of the Pd and Rh reference patterns. The mean lattice parameter, 3.857 Å, is also intermediate between the reference values for Pd and Rh. Vegard’s law gives an approximate composition of 38 at.% Rh (26–47 at.%, depending on the reflection used). This value depends on the peak fitting, the reference lattice parameters, the instrumental calibration and the assumption of a homogeneous substitutional solid solution, and should not be regarded as an independent quantitative measurement of composition.
These results are consistent with an fcc Pd–Rh solid solution but do not demonstrate homogeneity at the atomic scale; given the width of the reflections, a mixture of very small Pd-rich and Rh-rich domains cannot be ruled out. The crystallite size of about 3–4 nm, obtained from the Scherrer equation without correction for instrumental broadening, should be taken as an approximate coherent-domain size and not necessarily as the particle diameter. The sharp reflection at 26.5° (d ≈ 3.36 Å) is attributed to crystalline graphite in the conductive carbon tape used to mount the sample, since glassy carbon gives only a broad feature in this region.
Figure 6 compares the Pd 3d spectra of the Pd and Pd–Rh deposits and shows the Rh 3d spectrum of the Pd–Rh deposit. In both deposits the Pd 3d region contains metallic Pd together with several oxidized Pd components. In the Pd–Rh deposit, the Rh 3d region contains metallic Rh (Rh 3d5/2 = 307.46 eV) and Rh2O3 (308.86 eV). Only about 17% of the surface Pd signal of the Pd deposit, and about 8% of the Pd signal and 36% of the Rh signal of the Pd–Rh deposit, correspond to the metallic state, indicating extensive surface oxidation. The surface composition of the Pd–Rh deposit (C 67.7, O 10.6, Pd 12.1 and Rh 9.5 at.%) gives Rh/(Pd + Rh) ≈ 0.44, close to the 1:1 Pd:Rh ratio of the deposition bath and broadly consistent with the approximate Vegard estimate from XRD (about 38 at.% Rh), although XPS probes only the outermost few nanometres of the deposit.
The metallic Pd 3d5/2 binding energy is 335.57 eV for Pd and 335.50 eV for Pd–Rh. This difference (−0.07 eV) is within the uncertainty of the measurement, so the XPS data do not provide independent evidence of electronic interaction between Pd and Rh. Together, XRD and XPS support, but do not by themselves prove, the formation of a Pd–Rh solid solution. Atomic-scale analysis, for example scanning transmission electron microscopy with elemental line profiles across individual particles, would be needed to confirm homogeneous mixing.
Comparisons between materials are meaningful only when the experimental conditions are reported and controlled, since electrolyte composition, potential range, scan rate, electrode area, metal loading and test duration all affect the result. A higher current does not necessarily indicate higher catalytic activity; it may reflect a larger amount of deposited metal, a larger accessible surface or a competing reaction. Geometric current density and mass activity should therefore be reported, and specific activity only when the electrochemically active surface area has been determined by a suitable method. For CO₂ reduction, product identification and Faradaic efficiencies are essential, because the total current does not reveal which products are formed [1,4,6].
7. From Laboratory Measurements to Real-World Energy
A modified electrode is only the first step towards a sustainable technology. Assessing its potential usefulness requires data on activity, selectivity, durability and the energy demand of the complete system, as well as long-term tests under conditions close to practical operation.
Cost and resource use must also be considered. Palladium and rhodium are precious metals whose extraction and refining have significant environmental consequences. Lower metal loadings, better recycling and longer catalyst lifetimes can reduce this burden, provided that performance remains adequate. A complete device also includes supports, membranes, electrolytes, housing and power-management components.
The benefits of CO₂ conversion must be described with particular care, because converting CO₂ into a chemical product is not equivalent to removing it permanently from the atmosphere. If the product is used as a fuel, the carbon is released again when it is burned. The net climate effect depends on the origin of the CO₂, the electricity source, the energy used for capture and conversion, and the final fate of the product [28].
Sustainability therefore has to be assessed at the level of the whole process. A catalyst can be scientifically interesting without being economically viable or environmentally preferable to existing alternatives.
The recent literature also distinguishes between convenient handling properties and a lower life-cycle impact. A 2025 review of the environmental origin and fate of DESs noted that their carbon footprint, feedstock origin, toxicity and end-of-life behaviour are seldom reported, and recommended life-cycle assessment (LCA) to test sustainability claims [24]. A comparison between the choline chloride–urea route and an aqueous or conventional-solvent route should therefore use a common functional unit and account for heating, solvent preparation and recovery, rinse water, metal losses, waste treatment and the amount of usable catalyst obtained.
8. Green Chemistry, the 2030 Agenda and Circular Economy
Green chemistry offers a framework for evaluating whether the preparation and use of electrocatalysts can reduce environmental and health impacts. Its relevant principles include waste prevention, energy efficiency, the use of safer chemicals where technically possible and the design of processes with lower material losses. Electrodeposition from a choline chloride–urea deep eutectic solvent (DES) is an alternative preparation route, but using a DES does not in itself make the process environmentally benign. The route has to be evaluated in terms of the toxicity and sourcing of the solvent components, the energy needed for preparation and heating, solvent recovery and reuse, and the treatment of metal-containing residues, as summarized in Figure 7 [17,29].
Laboratory performance metrics can be combined with environmental indicators in a proportionate assessment. Useful measurements include the metal mass per geometric electrode area, the current normalized to metal mass or to electrochemically active surface area, product selectivity and Faradaic efficiency where applicable, long-term stability, metal leaching, solvent recovery yield, energy consumption per unit of deposited material, and the amount and classification of waste. For CO₂ conversion, the carbon source, electricity mix, separation requirements and final fate of the product should also be considered. A full life-cycle assessment becomes feasible once sufficient process data are available.
More electrochemical evidence is needed before application-level claims can be made. For an oxidation reaction, a minimum comparison should include the geometric current density, the mass activity referred to Pd or to the total metal, the specific activity normalized to the electrochemically active surface area when this can be reliably measured, the onset or peak potential on a clearly defined reference scale, and the durability under a stated protocol. The deposited metal mass and composition should be measured directly, since estimates from the deposition charge are valid only if the Faradaic efficiency is known. For CO₂ reduction, each product should be identified and its Faradaic efficiency, production rate and carbon balance reported. These data are required for a fair comparison of materials and to establish whether a gain in performance justifies the additional precious metal.
Circular-economy principles extend this analysis to the full life cycle of the catalyst and its preparation. Possible measures include recovering Pd and Rh from spent electrodes and process solutions, recovering and reusing the DES, reducing the consumption of rinse water and chemicals, and designing experiments that produce less hazardous waste. Each recovery route should itself be assessed in terms of energy demand, chemical inputs, yield and purity, since recycling is beneficial only if it brings a net environmental gain.
These considerations relate the present topic to the United Nations 2030 Agenda, in particular to Sustainable Development Goal (SDG) 7 (Affordable and Clean Energy), through more efficient energy-conversion systems; SDG 9 (Industry, Innovation and Infrastructure), through materials design and electrochemical manufacturing; SDG 12 (Responsible Consumption and Production), through resource efficiency, waste prevention and recycling; and SDG 13 (Climate Action), provided that a reduction in life-cycle greenhouse-gas emissions can be demonstrated [30]. These are potential contributions; they are not demonstrated by the microscopy, elemental analysis, voltammetry, diffraction or photoelectron spectroscopy data reported here.
The use of palladium and rhodium also raises questions of resource efficiency. Both metals have a high economic value, and their extraction and refining can carry a considerable environmental burden. Catalyst design should therefore aim at the lowest metal loading compatible with the required activity, selectivity and durability. Data on metal loading, dissolution during operation, recovery after use and the possibility of reusing the electrode or reclaiming the metals would show whether the approach actually reduces material demand or simply spreads precious metals over a larger surface.
Overall, the Pd–Rh deposits prepared in choline chloride–urea DES are best regarded as a materials-science case study that offers opportunities for more sustainable design, and not as evidence of a green or circular technology. These opportunities can be tested by comparing the DES route with suitable alternatives, with controls for metal loading and catalytic performance, and by measuring recovery, durability, energy use and waste. Such an approach keeps the scientific claims in line with the evidence and connects electrocatalysis research with green chemistry, the circular economy and the 2030 Agenda.
A logical next step is a controlled comparison of Pd, Rh and Pd–Rh prepared under identical conditions, together with a conventional-solvent control. This comparison should include direct measurements of metal loading and composition, replicate electrodes, dissolution tests after electrochemical use and an estimate of uncertainty. High-resolution elemental mapping or scanning transmission electron microscopy (STEM)–EDX line profiles would help to establish atomic-scale mixing, and operando or post-mortem characterization would show whether the initial structure is retained during use. These measurements would link the present mechanistic observations with catalytic performance and sustainability.
9. Conclusions
Pd- and Rh-containing nanomaterials are useful systems for studying how composition and surface structure affect electrochemical behaviour. Electrodeposition, including deposition from deep eutectic solvents, is a simple route for modifying conductive substrates, and microscopy, elemental analysis, electrochemical measurements, X-ray diffraction and photoelectron spectroscopy provide complementary information on the resulting materials. In the present case study, Pd appears to promote the co-deposition of Rh at potentials about 0.7 V less negative than those required for Rh alone, showing that combining metals can affect not only the final surface but also the way it forms.
Promising images or current curves should not be taken as proof of technological success. Reliable conclusions require appropriate controls, transparent reporting, product identification where relevant and stability tests that reflect the intended application.
Enzymes show what can be achieved when the environment around a metal centre is precisely controlled. Learning from them, while recognizing the practical limitations of both enzymes and nanomaterials, is a promising strategy for the design of better electrocatalysts.
Sustainable energy systems will not rely on a single metal or catalyst. They will require renewable electricity, efficient devices, responsible sourcing of materials, recycling and a realistic assessment of environmental impacts. Nanocatalysts are one component of this effort, and a better understanding of their surfaces will help to define the role of chemistry in future energy technologies.
Future studies should follow a staged approach: (i) establish reproducible synthesis, phase and composition; (ii) quantify catalytic activity and selectivity against monometallic and benchmark controls; (iii) determine durability and metal leaching; and (iv) compare environmental and economic performance using transparent process data and a defined functional unit. Following this sequence would allow the links with SDGs 7, 9, 12 and 13 to be supported by data.
Supplementary Materials
The following supporting information can be downloaded at the website of this paper posted on Preprints.org, Figure S1: Current–time transients recorded during potentiostatic deposition of Pd and Pd–Rh (−0.20 to −0.30 V) and Rh (−1.00 to −1.30 V) on glassy carbon from choline chloride–urea DES; Figure S2: Complete set of current–time transients for Rh between −0.98 and −1.30 V; Table S1: Maximum current density, deposited charge, equivalent metal mass and metal loading obtained from the transients; Table S2: Time of the current maximum of the transients; Figure S3: Current density at 5 s and charge passed during the transients as a function of the applied potential for Pd, Rh and Pd–Rh; Table S3: Peak potentials and current densities of the cyclic voltammograms in Figure 4.
Author Contributions
Conceptualization, V.A.M.R.; investigation, V.A.M.R. and M.G.M.O.Y.; formal analysis, V.A.M.R. and M.G.M.O.Y.; writing—original draft preparation, V.A.M.R.; writing—review and editing, M.G.M.O.Y.; supervision, M.G.M.O.Y. All authors have read and agreed to the published version of the manuscript.
Funding
This research received no external funding.
Institutional Review Board Statement
Not applicable.
Informed Consent Statement
Not applicable.
Data Availability Statement
The data supporting the findings of this study are available from the corresponding author upon reasonable request.
Acknowledgments
V. A. Medina Rojano gratefully acknowledges the Secretariat of Science, Humanities, Technology and Innovation (Secretaría de Ciencia, Humanidades, Tecnología e Innovación, SECIHTI), Mexico, for the doctoral scholarship granted. M. G. Montes de Oca Yemha acknowledges the National System of Researchers (Sistema Nacional de Investigadoras e Investigadores, SNII), Mexico, for membership and the associated stipend. During the preparation of this manuscript, the authors used Claude Opus 5.5 (Anthropic) for the purposes of linguistic editing and of redrawing Figure 7 from the authors’ draft, and Dream Lab (Canva) to generate draft versions of the graphical abstract and Figure 7, which were subsequently checked, edited and assembled by the authors using ImageJ (National Institutes of Health, Bethesda, MD, USA). The authors have reviewed and edited the output and take full responsibility for the content of this publication. The authors thank the Instituto Mexicano del Petróleo (IMP) for the XPS measurements and the Escuela Superior de Ingeniería Química e Industrias Extractivas (ESIQIE), Instituto Politécnico Nacional, for access to the SEM facilities.
Conflicts of Interest
The authors declare no conflicts of interest.
References
- Seh, Z.W.; Kibsgaard, J.; Dickens, C.F.; Chorkendorff, I.; Nørskov, J.K.; Jaramillo, T.F. Combining theory and experiment in electrocatalysis: Insights into materials design. Science 2017, 355, eaad4998. [Google Scholar] [CrossRef] [PubMed]
- Debe, M.K. Electrocatalyst approaches and challenges for automotive fuel cells. Nature 2012, 486, 43–51. [Google Scholar] [CrossRef] [PubMed]
- Jiao, Y.; Zheng, Y.; Jaroniec, M.; Qiao, S.Z. Design of electrocatalysts for oxygen- and hydrogen-involving energy conversion reactions. Chem. Soc. Rev. 2015, 44, 2060–2086. [Google Scholar] [CrossRef] [PubMed]
- Lee, C.-W.; Jung, S.Y.; Ryu, J.H.; Jeon, G.S.; Gaur, A.; Cho, M.S.; Ali, G.; Kim, M.; Chung, K.Y.; Nayak, A.K.; Shin, S.; Kwon, J.; Song, T.; Shin, T.H.; Han, H. Empowering Tri-Functional Palladium’s Catalytic Activity and Durability in Electrocatalytic Formic Acid Oxidation Reaction via Innovative Self-Caging and Alloying Strategies. Adv. Sci. 2024, 11, 2405725. [Google Scholar] [CrossRef] [PubMed]
- Gong, J.-X.; Hu, S.-Y.; Xiong, Y. Designing catalysts to formic acid oxidation reaction: From nanoscale to single atoms. J. Cent. South Univ. 2024, 31, 4586–4600. [Google Scholar] [CrossRef]
- Tan, X.; Wang, J.; Xiao, Y.; Guo, Y.; He, W.; Du, B.; Cui, H.; Wang, C. Engineering Topological and Chemical Disorder in Pd Sites for Record-Breaking Formic Acid Electrocatalytic Oxidation. Adv. Mater. 2025, 37, e2414283. [Google Scholar] [CrossRef] [PubMed]
- Qiao, Y.; Xie, Y.; Zhou, Y.; Yang, Y.; Feng, L. MOF-derived Pd/CeO₂-NC catalyst for efficient electrooxidation of formic acid. Chem. Commun. 2025, 61, 15421–15424. [Google Scholar] [CrossRef] [PubMed]
- Antolini, E. Palladium in fuel cell catalysis. Energy Environ. Sci. 2009, 2, 915–931. [Google Scholar] [CrossRef]
- Jiang, K.; Zhang, H.X.; Zou, S.; Cai, W.B. Electrocatalysis of formic acid on palladium and platinum surfaces: From fundamental mechanisms to fuel cell applications. Phys. Chem. Chem. Phys. 2014, 16, 20360–20376. [Google Scholar] [CrossRef] [PubMed]
- Min, X.; Kanan, M.W. Pd-catalyzed electrohydrogenation of carbon dioxide to formate: High mass activity at low overpotential and identification of the deactivation pathway. J. Am. Chem. Soc. 2015, 137, 4701–4708. [Google Scholar] [CrossRef] [PubMed]
- Kuhl, K.P.; Cave, E.R.; Abram, D.N.; Jaramillo, T.F. New insights into the electrochemical reduction of carbon dioxide on metallic copper surfaces. Energy Environ. Sci. 2012, 5, 7050–7059. [Google Scholar] [CrossRef]
- Lubitz, W.; Ogata, H.; Rüdiger, O.; Reijerse, E. Hydrogenases. Chem. Rev. 2014, 114, 4081–4148. [Google Scholar] [CrossRef] [PubMed]
- Reda, T.; Plugge, C.M.; Abram, N.J.; Hirst, J. Reversible interconversion of carbon dioxide and formate by an electroactive enzyme. Proc. Natl. Acad. Sci. USA 2008, 105, 10654–10658. [Google Scholar] [CrossRef] [PubMed]
- Fourmond, V.; Di Giuliantonio, A.; Malagnini, M.; Opdam, L.; Ostermann, N.; Webb, S.; Milton, R.D.; Léger, C. Direct Electrochemistry of Hydrogenase, Formate Dehydrogenase, CO Dehydrogenase, and Nitrogenase: Wiring Strategies and Mechanistic Insights into Metalloenzymes That Produce Solar Fuels. Chem. Rev. 2026, 126, 6550–6679. [Google Scholar] [CrossRef] [PubMed]
- Armstrong, F.A.; Hirst, J. Reversibility and efficiency in electrocatalytic energy conversion and lessons from enzymes. Proc. Natl. Acad. Sci. USA 2011, 108, 14049–14054. [Google Scholar] [CrossRef] [PubMed]
- Abbott, A.P.; Capper, G.; Davies, D.L.; Rasheed, R.K.; Tambyrajah, V. Novel solvent properties of choline chloride/urea mixtures. Chem. Commun. 2003, 70–71. [Google Scholar] [CrossRef] [PubMed]
- Smith, E.L.; Abbott, A.P.; Ryder, K.S. Deep eutectic solvents (DESs) and their applications. Chem. Rev. 2014, 114, 11060–11082. [Google Scholar] [CrossRef] [PubMed]
- Abbott, A.P.; Barron, J.C.; Frisch, G.; Gurman, S.; Ryder, K.S.; Silva, A.F. Double layer effects on metal nucleation in deep eutectic solvents. Phys. Chem. Chem. Phys. 2011, 13, 10224–10231. [Google Scholar] [CrossRef] [PubMed]
- Sebastián, P.; Botello, L.E.; Vallés, E.; Gómez, E.; Palomar-Pardavé, M.; Scharifker, B.R.; Mostany, J. Three-dimensional nucleation with diffusion controlled growth: A comparative study of electrochemical phase formation from aqueous and deep eutectic solvents. J. Electroanal. Chem. 2017, 793, 119–125. [Google Scholar]
- Juárez-Marmolejo, L.; Maldonado-Teodocio, B.; Montes de Oca-Yemha, M.G.; Romero-Romo, M.; Arce-Estrada, E.M.; Ezeta-Mejía, A.; Ramírez-Silva, M.T.; Mostany, J.; Palomar-Pardavé, M. Electrocatalytic oxidation of formic acid by palladium nanoparticles electrochemically synthesized from a deep eutectic solvent. Catal. Today 2022, 394–396, 190–197. [Google Scholar] [CrossRef]
- Ávalos-Huarte, E.; Montes de Oca-Yemha, M.G.; Medina-Rojano, V.A.; Romero-Romo, M.; Ramírez, C.; Morales-Gil, P.; Palomar-Pardavé, M. Electrochemical nucleation and growth of Pd–Ag alloy nanoparticles onto a bare and a conducting polymer-modified glassy carbon electrode from ethaline deep eutectic solvent. J. Solid State Electrochem. 2026, 30, 2249–2263. [Google Scholar] [CrossRef]
- Choi, Y.H.; van Spronsen, J.; Dai, Y.; Verberne, M.; Hollmann, F.; Arends, I.W.C.E.; Witkamp, G.-J.; Verpoorte, R. Are natural deep eutectic solvents the missing link in understanding cellular metabolism and physiology? Plant Physiol. 2011, 156, 1701–1705. [Google Scholar] [CrossRef] [PubMed]
- Dai, Y.; van Spronsen, J.; Witkamp, G.-J.; Verpoorte, R.; Choi, Y.H. Natural deep eutectic solvents as new potential media for green technology. Anal. Chim. Acta 2013, 766, 61–68. [Google Scholar] [CrossRef] [PubMed]
- Hayyan, M. The environmental origin and fate of deep eutectic solvents: A two-edged sword in sustainability claims. J. Mol. Liq. 2025, 439, 128928. [Google Scholar] [CrossRef]
- Wang, H.; Kang, X.; Han, B. Electrocatalysis in deep eutectic solvents: From fundamental properties to applications. Chem. Sci. 2024, 15, 9949–9976. [Google Scholar] [CrossRef] [PubMed]
- Maldonado-Teodocio, B.; Palomar-Pardavé, M.; Romero-Romo, M.; Ramírez, C.; Morales-Gil, P.; Torres-Rodríguez, M.; Montes de Oca-Yemha, M.G. Unraveling copper nucleation from Cu(I) in reline: Coupling thermodynamics, kinetics and interfacial structure. Metals 2026, 16, 668. [Google Scholar] [CrossRef]
- Sebastián, P.; Vallés, E.; Gómez, E. Copper electrodeposition in a deep eutectic solvent. First stages analysis considering Cu(I) stabilization in chloride media. Electrochim. Acta 2014, 123, 285–295. [Google Scholar]
- Mac Dowell, N.; Fennell, P.S.; Shah, N.; Maitland, G.C. The role of CO2 capture and utilization in mitigating climate change. Nat. Clim. Change 2017, 7, 243–249. [Google Scholar] [CrossRef]
- Anastas, P.T.; Warner, J.C. Green Chemistry: Theory and Practice; Oxford University Press: New York, NY, USA, 1998. [Google Scholar]
- United Nations. Transforming Our World: The 2030 Agenda for Sustainable Development; A/RES/70/1; United Nations General Assembly: New York, NY, USA, 2015. [Google Scholar]
Figure 1.
Morphological and elemental characterization of palladium-containing nanomaterials deposited on glassy carbon at −0.28 V for 60 s. (a) Scanning electron microscopy (SEM) image showing the distribution and morphology of predominantly spherical particles (10 kV, ×30,000 magnification; scale bar: 100 nm). (b) Energy-dispersive X-ray spectroscopy (EDX) spectrum showing signals attributed to carbon (C) and palladium (Pd). (c) Electron image of the mapped region. (d,e) EDX elemental maps of carbon and palladium, respectively, showing their spatial distribution across the analysed region (scale bars: 1 µm). The observations support the presence of Pd-containing particles on a carbon-containing material; further structural and quantitative analyses would be required to establish particle composition, crystallinity, and the degree of elemental dispersion.
Figure 1.
Morphological and elemental characterization of palladium-containing nanomaterials deposited on glassy carbon at −0.28 V for 60 s. (a) Scanning electron microscopy (SEM) image showing the distribution and morphology of predominantly spherical particles (10 kV, ×30,000 magnification; scale bar: 100 nm). (b) Energy-dispersive X-ray spectroscopy (EDX) spectrum showing signals attributed to carbon (C) and palladium (Pd). (c) Electron image of the mapped region. (d,e) EDX elemental maps of carbon and palladium, respectively, showing their spatial distribution across the analysed region (scale bars: 1 µm). The observations support the presence of Pd-containing particles on a carbon-containing material; further structural and quantitative analyses would be required to establish particle composition, crystallinity, and the degree of elemental dispersion.

Figure 2.
Morphological and elemental characterization of rhodium-containing nanomaterials deposited on glassy carbon at −0.28 V for 60 s. (a) Scanning electron microscopy (SEM) image showing clustered particles distributed across the substrate (10 kV, ×30,000 magnification; scale bar: 100 nm). (b) Energy-dispersive X-ray spectroscopy (EDX) spectrum showing signals attributed to carbon (C) and rhodium (Rh). (c) Electron image of the mapped region (scale bar: 2 µm). (d,e) EDX elemental maps showing the spatial distribution of carbon and rhodium, respectively (scale bars: 1 µm). The results support the presence of Rh-containing material in a carbon-containing region. Additional quantitative and structural characterization would be required to determine the Rh content, particle composition, crystallinity, and degree of elemental dispersion.
Figure 2.
Morphological and elemental characterization of rhodium-containing nanomaterials deposited on glassy carbon at −0.28 V for 60 s. (a) Scanning electron microscopy (SEM) image showing clustered particles distributed across the substrate (10 kV, ×30,000 magnification; scale bar: 100 nm). (b) Energy-dispersive X-ray spectroscopy (EDX) spectrum showing signals attributed to carbon (C) and rhodium (Rh). (c) Electron image of the mapped region (scale bar: 2 µm). (d,e) EDX elemental maps showing the spatial distribution of carbon and rhodium, respectively (scale bars: 1 µm). The results support the presence of Rh-containing material in a carbon-containing region. Additional quantitative and structural characterization would be required to determine the Rh content, particle composition, crystallinity, and degree of elemental dispersion.

Figure 3.
Morphological and elemental characterization of a Pd–Rh-containing material deposited on glassy carbon at −0.28 V for 60 s. (a) Scanning electron microscopy (SEM) image showing a dense distribution of faceted particles with substantial aggregation (10 kV, ×30,000 magnification; working distance: 7.2 mm; scale bar: 100 nm). (b) Energy-dispersive X-ray spectroscopy (EDX) spectrum showing signals attributed to carbon (C), palladium (Pd), and rhodium (Rh). (c) Electron image of the mapped region. (d–f) EDX elemental maps showing the spatial distributions of C, Pd, and Rh, respectively (scale bars: 1 µm). The results support the presence of Pd- and Rh-containing material in a carbon-containing region. Quantitative elemental analysis and additional structural characterization are required to determine the metal composition, establish whether a Pd–Rh alloy has formed, and assess the degree of elemental mixing.
Figure 3.
Morphological and elemental characterization of a Pd–Rh-containing material deposited on glassy carbon at −0.28 V for 60 s. (a) Scanning electron microscopy (SEM) image showing a dense distribution of faceted particles with substantial aggregation (10 kV, ×30,000 magnification; working distance: 7.2 mm; scale bar: 100 nm). (b) Energy-dispersive X-ray spectroscopy (EDX) spectrum showing signals attributed to carbon (C), palladium (Pd), and rhodium (Rh). (c) Electron image of the mapped region. (d–f) EDX elemental maps showing the spatial distributions of C, Pd, and Rh, respectively (scale bars: 1 µm). The results support the presence of Pd- and Rh-containing material in a carbon-containing region. Quantitative elemental analysis and additional structural characterization are required to determine the metal composition, establish whether a Pd–Rh alloy has formed, and assess the degree of elemental mixing.

Figure 4.
Cyclic voltammograms recorded on a glassy-carbon electrode (GCE) in choline chloride–urea DES containing (a) 50 mM PdCl₂, (b) 25 mM RhCl₃ and (c) 25 mM PdCl₂ + 25 mM RhCl₃, at scan rates of 10–50 mV s⁻¹. Potentials are referred to an Ag quasi-reference electrode (QRE); current densities refer to the geometric electrode area (0.196 cm²).
Figure 4.
Cyclic voltammograms recorded on a glassy-carbon electrode (GCE) in choline chloride–urea DES containing (a) 50 mM PdCl₂, (b) 25 mM RhCl₃ and (c) 25 mM PdCl₂ + 25 mM RhCl₃, at scan rates of 10–50 mV s⁻¹. Potentials are referred to an Ag quasi-reference electrode (QRE); current densities refer to the geometric electrode area (0.196 cm²).

Figure 5.
X-ray diffraction pattern of the Pd–Rh deposit prepared at −0.28 V (Cu Kα, λ = 1.5406 Å). (a) Full pattern with the reference reflections of Pd (PDF 46-1043) and Rh (PDF 05-0685). (b) Pseudo-Voigt fit of the (111) reflection; dashed lines mark the (111) positions of pure Pd and Rh, and the dotted line marks the fitted position.
Figure 5.
X-ray diffraction pattern of the Pd–Rh deposit prepared at −0.28 V (Cu Kα, λ = 1.5406 Å). (a) Full pattern with the reference reflections of Pd (PDF 46-1043) and Rh (PDF 05-0685). (b) Pseudo-Voigt fit of the (111) reflection; dashed lines mark the (111) positions of pure Pd and Rh, and the dotted line marks the fitted position.

Figure 6.
High-resolution XPS spectra with Shirley background and fitted components: (a) Pd 3d of the Pd deposit; (b) Pd 3d of the Pd–Rh deposit; (c) Rh 3d of the Pd–Rh deposit (glassy carbon, −0.28 V, 60 s). Binding energies are referenced to C 1s at 284.8 eV.
Figure 6.
High-resolution XPS spectra with Shirley background and fitted components: (a) Pd 3d of the Pd deposit; (b) Pd 3d of the Pd–Rh deposit; (c) Rh 3d of the Pd–Rh deposit (glassy carbon, −0.28 V, 60 s). Binding energies are referenced to C 1s at 284.8 eV.

Figure 7.
Framework linking the preparation of Pd–Rh electrodes in choline chloride–urea DES with laboratory and environmental sustainability metrics, circular-economy principles and potential contributions to SDGs 7, 9, 12 and 13 of the 2030 Agenda.
Figure 7.
Framework linking the preparation of Pd–Rh electrodes in choline chloride–urea DES with laboratory and environmental sustainability metrics, circular-economy principles and potential contributions to SDGs 7, 9, 12 and 13 of the 2030 Agenda.

Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content. |
© 2026 by the authors. Licensee MDPI, Basel, Switzerland. This article is an open access article distributed under the terms and conditions of the Creative Commons Attribution (CC BY) license.
Copyright: This open access article is published under a Creative Commons CC BY 4.0 license, which permit the free download, distribution, and reuse, provided that the author and preprint are cited in any reuse.