Submitted:
29 October 2026
Posted:
30 October 2026
You are already at the latest version
Abstract
Dry drilling of autoclave-cured GLARE 3-3/2 laminates was investigated with rolled and ground high-speed-steel drills (HSS-R, HSS-G) and a carbide-tipped drill in a 3³ full factorial design (715, 1520 and 3030 rpm; 0.1, 0.2 and 0.3 mm/rev). Thrust force, infrared temperatures and the non-contact topography of the entry and exit faces were recorded for every hole, and sectioned hole walls were examined by scanning electron microscopy. Drill type governed the thrust force (29.6% contribution; 33.3 N for HSS-G versus 39.5 N for carbide), whereas feed governed the maximum drill temperature (38%; 101.5–114.6 °C); workpiece temperatures stayed below 43 °C, so thermal damage of the epoxy layers can be excluded. Exit burrs dominated over entry damage (mean burr height −3.9 μm at entry versus +25.7 μm at exit; p < 0.001). The carbide drill produced the most accurate holes but the largest exit burrs (up to 152 μm), the HSS-R drill produced bell-mouthed entries (+0.30 mm), and the HSS-G drill produced the flattest edges. Hole walls showed fibre pull-out, matrix chipping and interfacial debonding with HSS-R but transverse fibre shearing with carbide. Contribution analysis of 81 replicated measurements showed that exit-edge quality is governed by drill-specific speed–feed interactions. Response-surface modelling with a weighted desirability function and exhaustive grid search identified HSS-G at 1520 rpm and 0.2 mm/rev as the best compromise (D = 0.867; thrust force 31.1 N; exit burr height 1.8 μm; bulging ratio 0.8%).
Keywords:
GLARE
; fibre metal laminate
; dry drilling
; thrust force
; burr height
; bulging ratio
; scanning electron microscopy
; response surface methodology
; desirability function
1. Introduction
Fibre metal laminates (FMLs), in which thin metal sheets alternate with fibre-reinforced polymer (FRP) layers, combine the ductility of aluminium with the specific strength and fatigue resistance of composites [1]. GLARE (glass laminate aluminium reinforced epoxy), developed at Delft University of Technology and applied in the Airbus A380 fuselage, is the commercially most successful FML [2,3,4,5]: fibre bridging slows crack growth in the aluminium layers and improves the fatigue resistance and damage tolerance of the laminate [6,7,8]. Its production chain, from lay-up and curing to drilling and mechanical assembly, was described by Sinke [9], and the role of metal surface preparation was recently reviewed by Caggiano et al. [10].
Drilling is the most defect-prone step in the manufacture and repair of GLARE structures, because the aluminium and composite layers differ in cutting mechanics, thermal properties and damage modes. Recent reviews cover the machinability and sustainability of FMLs [11], one-shot drilling of FRP/aluminium stacks [12], machining of carbon-, glass- and natural-fibre composites [13], bibliometric trends in composite drilling [14], drilling of FRP [15], damage mechanisms in milling and grinding [16], advanced tools and coolants [17], finite-element modelling of composite machining [18] and the influence of hole quality on joint strength [19]. In a related study from the same laboratory, Ürgün et al. [20] combined thrust-force measurement, infrared thermography, optical profilometry and SEM with factorial ANOVA to study dry drilling of carbon/glass-epoxy laminates on the same bench drilling machine.
Drilling-induced delamination occurs when the axial thrust force exceeds the interlaminar strength of the laminate. The fracture-mechanics model of Hocheng and Dharan [21] treats exit push-out and entry peel-up as separate events [22], and the delamination factor of Chen [23] remains the most common damage metric. Later work addressed the critical thrust force of different drill geometries [24,25], image-based delamination factors [26,27], the assessment and suppression of delamination [28,29] and the role of the chisel edge and step-drill geometry [30]; Ürgün et al. [20] showed experimentally that a stepped cutting profile produces a non-monotonic dependence of thrust and temperature on drill diameter.
Experimental work on GLARE drilling is dominated by the studies of Giasin et al., who quantified the effects of cutting speed and feed on thrust force, torque, roughness, burr formation, hole size and delamination [31,32], validated finite-element force predictions [33], and examined tool coatings [34,35], cryogenic and minimum-quantity-lubrication cooling [36,37] and ultrasonic assistance [38]. Other studies addressed force, torque, acoustic emission and delamination [39], drilling versus helical milling [40], special drill geometries [41], process forces and temperature fields [42], hole quality and dust emission in GLARE 2B [43], HSS-Co versus carbide drills [44], CARALL laminates [45], Taguchi-based and machine-learning optimisation [46,47], regression modelling [48], ultrasonic-assisted drilling from the tool-design and simulation viewpoints [49,50], grey relational optimisation [51] and helical milling of CARALL [52].
Abrasive water-jet drilling has been proposed as an alternative to conventional drilling of GLARE [53,54,55]. Infrared thermography, as used here, was applied to GLARE drilling by Giasin and Ayvar-Soberanis [56] and by Ürgün et al. [20]; the merits of thermocouple and infrared measurements [57], the temperatures developed in CFRP drilling and their effect on the constituents [58,59,60] and the heat partition in CFRP cutting [61] have also been reported.
Design-of-experiments and optimisation techniques are widely used in composite and FML machining. Response-surface methodology (RSM) [62,63] combined with the desirability function of Derringer and Suich [64] is the standard multi-response approach and has been applied to burr height in drilling of aluminium-matrix composites [65,66], whereas FML drilling has relied mainly on Taguchi-based grey relational analysis [46,51]. Taguchi, regression and utility-theory approaches to GFRP and CFRP drilling [67,68,69,70,71], evolutionary multi-objective algorithms [72], force–delamination correlations [73,74], nanocomposite milling [75] and numerous milling optimisation studies [76,77,78,79,80,81,82,83] follow the same pattern. Work on hybrid metal–composite stacks [84,85,86,87], tool wear and coatings [88,89], ultrasonic-assisted milling [90], Kevlar/epoxy milling [91], hand laid-up hybrid laminates [92] and trimming-induced damage [93] provides further insight into the behaviour of the metal–composite interface.
Most of these studies consider a limited number of responses and describe hole damage with two-dimensional metrics such as the delamination factor or the wall roughness. Few studies measure the three-dimensional topography of both the entry and exit faces, fewer combine face metrics with SEM of the wall damage, and none compares rolled HSS, ground HSS and carbide-tipped drills for GLARE 3-3/2 under dry conditions in a full factorial design with the categorical drill type included in a multi-objective optimisation. The present study therefore (i) measures the thrust force and the workpiece, chip and drill temperatures for three drills, three spindle speeds and three feeds; (ii) quantifies the entry and exit topography by non-contact profilometry and derives threshold-free aperture and edge metrics, namely burr height and bulging ratio; (iii) characterises the damage of the aluminium sheets, glass plies and adhesive layers on the hole walls by SEM; (iv) ranks the main and interaction effects by ANOVA and contribution analysis of replicated data; (v) identifies the best compromise of drill type, speed and feed by RSM, a weighted desirability function and exhaustive grid search; and (vi) derives practical recommendations for dry drilling of GLARE 3-3/2.
2. Materials and Methods
2.1. GLARE 3-3/2 Laminate
The GLARE 3-3/2 laminates consist of three plies of the 7075-T6 aluminum alloy material (thickness 0.41 mm [0.016 in]; part no. 7075T6-016x48x144AP) sandwiched together with two plies of glass fiber/epoxy composite material between them. The composite layers include E-glass prepreg cloth certified according to Boeing BMS 8-139 Class I standard (Style 1581, lot 92M0103414-031, Heatcon Composite Systems; and Style 120, part no. BMS 8-139 120 38 CL1, lot 92M0104198-013, Pacific Coast Composites) having the nominal weight percent of the resin content 36% in Style 1581 according to the vendor data [94].
Table 1.
Constituents of the GLARE 3-3/2 laminate.
| Layer | Material | Specification / part no. | Thickness |
| Aluminium sheets (×3) | 7075-T6 | 7075T6-016x48x144AP | 0.41 mm (0.016 in, nominal) |
| Glass/epoxy layers (×2) | E-glass prepreg, Style 1581 (36 wt % resin) and Style 120 | BMS 8-139 Class I (Heatcon / Pacific Coast Composites) | [layer thickness / number of prepreg plies per layer] |
| Adhesive | 3M Scotch-Weld AF 163-2 film adhesive | — | — |
| Cure | Autoclave, 105 ± 5 °C, 6 h, 1.2 bar, vacuum 0.15 bar | Airbus SRM 53-15-12 | Total 2.55 mm (digital caliper) |
The aluminum sheets were prepared by cutting them to required sizes and treating them with a degreasing process and primer treatment. Then, the sheets were bonded using 3M Scotch-Weld AF 163-2 film adhesive and laminated using the prepreg layers. The laminating process included applying the peel ply and breather to the lay-up and vacuum-bagging and curing of the lay-up in an autoclave according to the cycle recommended for the GLARE panels in the Airbus Structural Repair Manual 53-15-12 [95]. The curing cycle consisted of a vacuum of 0.15 ± 0.05 bar, autoclave pressure increase to 1.2 bar with steps, heating to 105 ± 5 °C at 1.5 °C/min, and 6-hour dwell.
2.2. Drilling Set-Up and Experimental Design
The dry drilling operations were performed on a Toss United TU5032B bench drilling machine. This machine is equipped with fixed steps of spindle speeds due to step-pulley drive, and mechanical feed increments of 0.1, 0.2, and 0.3 mm/rev. The same machine was used in the related work by Ürgün et al. [20] because of the stable cutting conditions. The 3 × 3 × 3 full-factorial design was designed using three different spindle speeds (715, 1520, and 3030 rpm), three feed rates (0.1, 0.2, and 0.3 mm/rev) and three different drill types resulting in 27 conditions. The specimens were clamped into the fixture mounted to the dynamometer that in turn was clamped to the machine table. The three drills that were tested in this work were: (a) rolled (not ground) DIN 338 high-speed-steel twist drill (HSS-R, Ø6.00 mm), (b) completely ground DIN 338 high-speed-steel twist drill (HSS-G, Ø6.00 mm), and (c) carbide tipped twist drill with Ø6.35 mm (1/4 in) diameter. All the drills had a point angle of 118°. Every drill was a new one and was used for drilling nine holes in its group, and no noticeable wear of cutting edges was found after nine holes. The whole data set is represented by three independent experimental sets (N = 3) that correspond to the 3 × 3 × 3 design (81 observations). In each set, the different drills of each type and different specimens were used. The first experimental set (odd specimens E1–E53, 27 holes; Table 2) was used for the hole-by-hole analysis that is described in Section 3.1, Section 3.2, Section 3.3, Section 3.4 and Section 3.5, and all three experimental sets were used in the contribution analysis and multi-objective optimization that is described in Section 3.6 (means for the conditions are presented in Table S1).
2.3. Thrust Force and Temperature Measurement
The axial thrust force was measured using a Kistler 9272 four-component piezoelectric dynamometer and a charge amplifier Kistler 5070A. Data acquisition was done with the use of DynoWare 2825D-02. For each hole the following parameters were calculated: mean thrust force (Fmean) and maximum thrust force (Fmax). Torque was not measured. Drilling zone temperature was measured simultaneously using a FLIR A325sc infrared camera (320 × 240 pixels, 7.5–13 μm) placed 50 cm away from the workpiece and oriented to 60° from it with recordings analyzed using FLIR ResearchIR software; such an arrangement was applied also by Ürgün et al. [20]. For each hole the temperature of the workpiece surface at two different points (Tw), mean and maximum chip temperature (Tchip) and maximum drill temperature (Tmax) were determined. Moreover, single images obtained at the moment of drill withdrawal were analyzed under certain conditions (see Section 3.2). Emissivity value applied in the camera software is not provided; therefore the reported temperatures can be treated as apparent temperatures only.
2.4. Hole-Edge Topography at the Entry and Exit Faces
Quantification of topography of entrance (drill entry) and exit (drill breakout) was done with a Nanovea PS-50 optical profilometer (non-contact chromatic confocal sensor). In each hole, scanning of 10 mm × 10 mm square area centered around the hole was performed with lateral step size of 15 μm in x direction and 20 μm in y direction, resulting in 668 × 501 height points for each face. Leveling of height maps was done by least-squares fitting of a flat surface in an undamaged annulus between 4.2 and 4.9 mm radii from the center of the hole, after 3σ outlier rejection, which results in a relative height profile with respect to the intact surface of the sheet. No signal was detected for points falling in the through-hole or almost vertical walls, and the largest non-scanned area in such a map defines the aperture of the hole. From this aperture, area (A), equivalent diameter (Deq = 2(A/π)1/2), and out-of-roundness (Dmax − Dmin) were calculated.
Edge quality was assessed in the annular zone from 0 to 300 µm away from the hole boundary using: (i) the average circumferential height profile derived from measurements of 180 radial rays, with each one oriented to its crossing point with the boundary; (ii) the burr height (BH), which is the average height of the first 60 µm of the surface adjacent to the wall (with positive BH meaning a raised burr, while negative indicates a rolled or chipped edge) denoted BHin and BHout on entry and exit edges respectively; (iii) the bulging ratio (BR), which is the percentage of the band above 40 µm relative to the reference plane, i.e., the circumferential dimension of the bulge of the sheet at the hole edge [21,96], as well as the depressed fraction (DF), that is, the percentage of the band located below 40 µm relative to the reference plane. In addition, the surface descriptors ‘Hole’ and ‘Peak’ measured by the software of the instrument (Professional 3D 6.2, ISO 25178 particle analysis) were also evaluated for comparative purposes. Areal roughness parameters Sa and Sz were not used as hole-quality measures because they are dominated by the aperture itself in a through-hole scan.
2.5. Scanning Electron Microscopy of the Hole Walls
After profilometric measurement, twelve samples from the first set of holes were cut along the plane cutting the hole axis and their walls were inspected using a JEOL JSM-6060 scanning electron microscope (SEM) operated at 15 kV acceleration voltage and a working distance of 24 mm. Holes drilled with rolled high-speed steel (HSS) and carbide drill at 0.1 and 0.3 mm/rev feed rates and at the three spindle speeds were chosen (E1, E13, E19, E31, E37, and E49 for HSS-R; E5, E17, E23, E35, E41, and E53 for carbide; Table 2). These correspond to the two drills having the most contrasting entry- and exit-face characteristics at the two extreme feed rates. The ground HSS drill was not considered in the SEM investigations. For each hole, an overall BES micrograph (×20 magnification) of the hole wall was taken, followed by BES images at ×100 magnification in several positions across the thickness. Additional SEI images were made for the carbide hole at 715 rpm/0.1 mm/rev. In BES images, Z-contrast allows for distinguishing 7075-T6 sheets (white), glass-fibre plies (light grey with identifiable fibre bundles), and epoxy-rich adhesive interlayers (dark grey). This makes it possible to identify layer boundaries, aluminium shavings and glass fibres without etching. Damage characteristics were described as feed marks, aluminium sheet ploughing and smearing, fibre pull-out, fibre fracture, matrix smearing, matrix chip-off or tearing, interfacial delamination and adhered chips and debris, following the classification used for FRP and FML hole walls [11,12,15,16].
2.6. Statistical Analysis and Multi-Objective Optimisation
Responses in the initial experiment were subjected to analysis by the three-factor ANOVA with fixed categorical factors of drill type, spindle speed, and feed, as well as the three two-factor interactions. Due to the unreplicated nature of this design, the three-factor interaction played the role of the error term in the test statistics, and the type-II sums of squares provided percentage contributions to the sum of squares of each term. As for edge quality measures that demonstrated severe skewness, the non-parametric Kruskal–Wallis test and Wilcoxon signed-rank test were applied. Correlations between the responses were measured by Pearson and Spearman methods. The significance level was set at α = 0.05. All computations were made using Python 3.11 (statsmodels 0.14, SciPy 1.11).
For the replicated data (N = 81) the complete 3^3 design, including the three-factor interaction, was used, with 54 degrees of freedom for the error term and contribution of each term expressed in terms of its percentage of the total sum of squares. Pooled second-order response-surface models [62,63] with intercepts specific to each drill were estimated next. The optimal settings of drill type, spindle speed, and feed were obtained by maximizing a weighted desirability function [64] through exhaustive grid search and leave-one-condition-out cross-validation, stratified bootstrap resampling [97], other weighting schemes, and weighted-sum score [98]. The method is outlined in Section 3.6. Computation was done using Python 3.12.3 (NumPy 2.4.4, SciPy 1.17.1, pandas 3.0.2, Matplotlib 3.10.8).
3. Results and Discussion
3.1. Thrust Force
The mean and peak thrust forces of the 27 holes are listed in Table 2 and plotted in Figure 1a,b. The mean thrust force ranged from 28.5 N (HSS-G, 1520 rpm, 0.1 mm/rev) to 44.0 N (carbide, 715 rpm, 0.2 mm/rev), and the peak force exceeded the mean by only 0.4–2.6 N, indicating a stable cut without force spikes at the aluminium/composite interfaces. The drill averages were 33.3 ± 5.6 N (HSS-G), 36.9 ± 3.1 N (HSS-R) and 39.5 ± 3.1 N (carbide). The two highest HSS-G values (43.6 N in E9 and 41.9 N in E45) coincided with chip packing around the drill point; without them the HSS-G mean falls to 30.6 N, 17% below HSS-R and 23% below carbide. The higher thrust of the carbide drill is attributed to its larger diameter (6.35 versus 6.00 mm, i.e. a 12% longer chisel edge) and to the less acute cutting edge of a wear-resistant carbide grade.
The ANOVA (Table 3) identifies drill type as the only significant factor for the mean thrust force (p = 0.014 in the main-effects model; 29.6% contribution), whereas spindle speed (8.4%), feed (6.9%) and the interactions are not significant. The main-effect plots (Figure S1a) show a shallow minimum at 1520 rpm and a maximum at 0.2 mm/rev, but these effects (about 3 N) are comparable with the residual scatter. The weak feed effect, in contrast to CNC drilling of thicker GLARE [31,32,43], is explained by the small laminate thickness (2.55 mm, of which only 1.2 mm is aluminium), so that the chisel edge never engages more than one layer at a time, and by the mechanically coupled feed of the bench drilling machine. The thrust forces (28–44 N) are far below the 150–500 N reported for 6 mm holes in 3–5 mm thick GLARE [31,42,44].
3.2. Thermal Response
The maximum drill temperature (Figure 1c) ranged from 84 to 123 °C and was practically independent of drill type (107.1–107.4 °C; p = 0.99), but increased steadily with feed (101.5, 105.7 and 114.6 °C at 0.1, 0.2 and 0.3 mm/rev; p = 0.003; 38% contribution) and peaked at the intermediate speed (103.0, 111.3 and 107.6 °C at 715, 1520 and 3030 rpm; p = 0.069; Figure S1b). The feed effect reflects the larger amount of heat generated per revolution, whereas the non-monotonic speed effect results from the competition between a higher frictional heating rate and a shorter drilling time (2.1 s at 715 rpm/0.1 mm/rev versus 0.2 s at 3030 rpm/0.3 mm/rev), which limits conduction into the drill body; similar behaviour was reported by Ürgün et al. [20] and by Giasin and Ayvar-Soberanis [56].
The chip temperature (Figure 1d) showed the widest range (26–86 °C) and depended on the drill × speed interaction (p = 0.018; 45.5% contribution; Table 3) rather than on the main effects, in line with the chip morphology: long continuous aluminium ribbons wrapped around the drill retain heat, whereas short segmented chips cool before being imaged. The workpiece surface temperature remained low (24–43 °C, mean 30 °C), differed slightly between drills (27.2, 30.8 and 32.0 °C for HSS-R, HSS-G and carbide; p = 0.038) and correlated with the mean thrust force (r = 0.62), i.e. a larger share of the ploughing energy heats the workpiece with the duller tool. No workpiece temperature approached the glass transition temperature of the epoxy matrix (120 °C for a 120 °C-curing system) or of the AF 163-2 adhesive, so thermal degradation of the interfaces can be excluded; the drill body, however, reached 112–123 °C at 0.3 mm/rev, which for HSS tools calls for lubrication or intermittent cooling at higher feeds or hole counts [57,58]. Thermograms recorded at drill withdrawal at 715 rpm (Figure S2) illustrate the local character of the temperature field around the drill, chips and workpiece; because the single-frame drill temperatures are far below the maxima of the complete records, they are used only for visualisation (Supplementary Note S1).
3.3. Entry- and Exit-Face Hole-Edge Quality
Figure 2 shows the circumferentially averaged height profiles of the entry face (upper half of each panel) and the exit face (lower half), which together form a schematic through-thickness section of the hole edge. Three trends emerge. First, the burr was always larger at the exit than at the entry face (mean burr height −3.9 µm versus +25.7 µm; Wilcoxon signed-rank test, p = 0.0002, n = 26): in the 3-3/2 lay-up the breakout of the bottom 7075-T6 sheet, supported only by the thin glass/epoxy layer, determines the burr size, in agreement with the push-out mechanism [21] and with Giasin and Ayvar-Soberanis [32] and Park et al. [44]. Second, the HSS-G entry faces were the flattest (BHin = 1.6 ± 10.2 µm; no hole beyond ±20 µm), whereas the HSS-R and carbide drills left raised (E1, E19; E5, E11, E17, E29) or rolled-over/chipped (E25, −75 µm; E47, −92 µm; E49 and E53, −25 µm) entry edges. Third, the carbide exit profiles peak 50–150 µm above the bottom face within 100 µm of the wall and decay over about 0.3 mm, whereas the HSS exit profiles stay within 0–40 µm.
Figure 3 compares the burr heights, bulging ratios and depressed fractions of the 0–300 µm edge band hole by hole. On the exit face the carbide drill produced the largest burrs (BHout = 152, 91, 75 and 58 µm for E35, E23, E17 and E29; group mean 39 ± 68 µm) and the highest bulging ratio (BRout = 22.4% versus 6.1% for HSS-R and 3.7% for HSS-G; Kruskal–Wallis, p = 0.0009; ANOVA, drill type p = 0.003, 57.8% contribution, Table 3). Its exit burr was strongly parameter dependent: the four largest burrs occurred at 1520 rpm (mean BHout = 100 µm) or at 0.3 mm/rev (87 µm), whereas at 3030 rpm BHout fell to 1.5 µm on average. The carbide drill generates the largest thrust (Section 3.1), and a larger axial load on the last sheet favours plastic push-out over clean shearing [32,44]; at 3030 rpm the higher strain rate and local temperature shear the thin sheet before it bends. The two HSS drills gave similar exit burrs (18.9 ± 17.6 µm for HSS-R and 18.4 ± 9.1 µm for HSS-G), but the ground drill was twice as repeatable and had the smallest bulging ratio. Over the 26 regular holes the mean thrust force and BHout were uncorrelated (Pearson r = −0.11, p = 0.61), so tool geometry rather than force governs the burr morphology, as also found by Giasin et al. [34]; BHout and BRout were positively correlated (r = 0.68; r = 0.86 with E9 included).
Depressed and raised entry edges occurred with similar frequency (mean DFin = 3.1–4.0% for all drills); the strongest entry rounding was found for HSS-R at 1520 rpm/0.2 mm/rev (E25; DFin = 10.3%) and for carbide at 3030 rpm/0.2 mm/rev (E47; DFin = 17.1%). These defects correspond to peel-up [21,22]: the thin top sheet (0.41 mm) is lifted along the flute helix before it is sheared, which is aggravated by the wandering chisel edge of the rolled drill and by the rapid feed of the rigid carbide drill at high speed.
The levelled height maps in Figure 4 (1520 rpm/0.1 mm/rev and the chip-clogged hole E9) illustrate these differences: the HSS-G hole is round and burr-free on both faces, the HSS-R hole is enlarged and rounded at the entry, and the carbide hole carries an asymmetric exit burr ring typical of the push-out of the last sheet when only one cutting lip carries the load. In E9 the exit sheet is bent around the whole circumference and a chip fragment adheres to the edge.
The HSS-G hole E9 (715 rpm, 0.2 mm/rev) suffered chip clogging at the drill point, which deformed the exit face severely (Figure 2, dashed curve of the HSS-G group; Figure 4): BHout = 245 µm, BRout = 85%, out-of-roundness 4.0 mm and an aperture area of 38.5 mm² (equivalent diameter 7.0 mm instead of 5.98 mm for the other HSS-G holes). Its entry face was normal (BHin = 21 µm), but its thrust force (43.6 N) and chip temperature (85 °C) were the highest of the HSS-G group. The event shows that in dry drilling of GLARE the exit quality depends on chip evacuation as much as on the nominal parameters: continuous 7075-T6 chips can weld to the flutes of an uncoated HSS drill at low speed and turn it into a punch [12,32]. E9 is therefore reported but excluded from the group statistics of Section 3.3 and Section 3.5.
The equivalent diameter of the non-measured aperture is a threshold-free measure of the through-hole size at each face (Figure S3a), expressed as oversize relative to the nominal drill diameter (6.00 mm for HSS, 6.35 mm for carbide). The three drills differed significantly (Kruskal–Wallis, p < 0.001; Table 4). The carbide drill gave the most accurate apertures (+25 ± 42 µm at entry, −7 ± 17 µm at exit) owing to its stiffness and precision grinding; the HSS-G drill was nearly as accurate (−8 ± 38 µm and −19 ± 40 µm, slightly undersize because of the elastic recovery of the sheets); the HSS-R drill produced an enlarged entry aperture (+301 ± 166 µm, up to +0.48 mm) but a near-nominal exit (+38 ± 40 µm), i.e. a bell-mouthed hole caused by run-out and the poor self-centring of the unground point in thin sheets [35]. The exit out-of-roundness (Figure S3b) was similar for the three drills (394–450 µm), showed no systematic dependence on speed or feed and was governed by local burrs and chip fragments at the boundary. The instrument-reported ‘Hole’ and ‘Peak’ areas did not discriminate between the entry and exit faces (Wilcoxon test, p = 0.22 and 0.24) because they rely on a scan-relative height threshold (Figure S4; Supplementary Note S2).
3.4. Hole-Wall Morphology
Figure 5 presents the BES overviews of the twelve sectioned holes (rows: drill and feed; columns: speed). The five-layer structure (three bright 7075-T6 sheets and two glass/epoxy layers, each consisting of a light grey fabric ply between two dark, epoxy-rich adhesive layers) is resolved in every image, and the 20–60 µm dark round features in the adhesive layers are pores of the AF 163-2 film revealed by sectioning, not drilling damage. The two drills produced clearly different walls. The HSS-R holes (Figure 5a–f) show irregular, fibre-covered glass/epoxy layers, ragged top-sheet edges at 1520 rpm/0.1 mm/rev and 715 rpm/0.3 mm/rev (Figure 5b,d), a lifted chip fragment at 3030 rpm/0.1 mm/rev (Figure 5c), a burr lip at 1520 rpm/0.3 mm/rev (Figure 5e) and local tearing and smearing of the middle sheet at 3030 rpm/0.3 mm/rev (Figure 5f). The carbide holes (Figure 5g–l) show uniform, continuous layers with straight sheet/composite boundaries; the only macroscopic defects are loose fibre fragments at 715 rpm/0.3 mm/rev (Figure 5j) and, at 1520 rpm/0.3 mm/rev (Figure 5k), two zones where the top sheet bent away from the composite and debonded from the adhesive over several hundred micrometres. This is the hole with the largest exit burr of the series (E35; BHout = 152 µm, BRout = 41.5%): the last sheet was pushed out by the chisel edge and bent before being sheared, as described by the push-out model of Hocheng and Dharan [21].
At ×100 (Figure 6) the HSS-R walls display circumferential feed marks on the aluminium (Figure 6a), a ploughed and torn surface with adhering debris at 1520 rpm/0.1 mm/rev (Figure 6c) and aluminium smeared over the adjacent adhesive at 3030 rpm/0.3 mm/rev (Figure 6f). The fibres are not cut cleanly: bundles parallel to the wall are pulled out (Figure 6a,d,e), transverse bundles are crushed into fragments lying on the wall (Figure 6a–c,e), and the matrix between them is smeared or stripped. In the adhesive interlayers the resin is torn out in chunks at 1520 rpm (Figure 6c,d), an aluminium chip fragment is welded to the wall at 715 rpm/0.3 mm/rev (Figure 6b), and at 3030 rpm/0.3 mm/rev the adhesive peels away from the middle sheet over more than 0.5 mm (interfacial debonding, Figure 6f). These features are typical of an edge that bends and breaks the fibres instead of shearing them: the rolled drill has an unground, rounded edge and a thick web, as reported for blunt or worn tools in FRP drilling and trimming [15,16,88]. Increasing the feed from 0.1 to 0.3 mm/rev shifts the damage from the plies to the interfaces (matrix chipping, aluminium smearing and debonding), consistent with the higher chip load per lip and the higher drill temperature at 0.3 mm/rev (Section 3.2), whereas increasing the speed did not clean the HSS-R wall, in contrast to its effect on the exit burr (Section 3.3).
The carbide walls (Figure 7) show a cutting-dominated process: small regular feed marks without ploughing (Figure 7a,e,f), clean and straight sheet/composite boundaries (Figure 7a), transversely sheared fibre ends flush with the wall (Figure 7a,c,e,f) and a thin glossy film of smeared resin partly covering them (Figure 7a,d), with few loose particles. Three departures are informative. At 715 rpm/0.3 mm/rev (Figure 7b), the lowest cutting speed (14.3 m/min) combined with the highest chip load, the aluminium at the sheet boundary is smeared and flaked over the adjacent layer and the adhesive is flaked. At 1520 rpm/0.3 mm/rev (Figure 7d) the fabric ply is broken into fine fragments, the smeared matrix is cracked and the composite layer protrudes above the aluminium (interface step), indicating softening and displacement of the adhesive. At 3030 rpm and 0.1 or 0.3 mm/rev (Figure 7e,f) a chipped adhesive fragment and a bright aluminium film smeared over the composite are seen. Aluminium particles and smears on the composite wall (Figure 7c,f) originate from chips carried by the flutes into the softer layers, as is typical of dry one-shot drilling of metal–composite stacks [12,87].
The SEM observations complement the profilometry in three respects. First, the ranking of the two drills reverses between the hole faces and the hole wall: the carbide drill, which produced the largest exit burrs and bulging ratios (Section 3.3), gave the cleanest walls, whereas the rolled HSS drill, whose exit burr never exceeded 40 µm, produced fibre pull-out, matrix chipping and interfacial debonding. The exit burr is a plastic-bending defect controlled by the axial load and the drill rigidity, whereas wall damage is a cutting defect controlled by edge sharpness; a sharp, stiff carbide edge reduces the latter and increases the former, in agreement with Giasin et al. [34] and Park et al. [44]. Second, the glossy matrix and the cracked or displaced adhesive at 0.3 mm/rev reflect the drill temperatures of 112–123 °C at that feed (Section 3.2), close to the glass transition of a 120 °C-cured epoxy: although the bulk workpiece stays below 43 °C, the wall is heated locally by the tool margin, as discussed by Merino-Pérez et al. [58,59] for CFRP. Third, the aluminium fragments welded to or smeared over the composite (Figure 6b and 7c,f) and the lifted chip fragment at 3030 rpm (Figure 5c) are the wall counterpart of the chip-evacuation problem observed at the exit face, as reported for GLARE [32] and FRP/aluminium stacks [12], and support the use of peck drilling or through-tool air at these feeds. Together with the flat entry edges and accurate apertures of Section 3.3, the SEM results show that a sharp, symmetrically ground cutting edge is the primary requirement for damage-free dry drilling of thin GLARE. The SEM study was qualitative, covered twelve of the 27 holes and did not include the HSS-G drill, so the wall morphology at the optimum condition of Section 3.6 (HSS-G, 1520 rpm, 0.2 mm/rev) remains to be verified.
3.5. Relations Between Force, Temperature and Edge Quality
Neither the mean thrust force nor the maximum drill temperature predicts the exit burr across drill types (Figure S5): the largest burrs were produced at thrust forces (36.8–40.7 N) and drill temperatures (107–120 °C) at which the HSS holes were burr-free. Within the HSS-R group, however, BHout decreased with increasing thrust force (Spearman ρ = −0.69, p = 0.038), i.e. the most aggressive cut at 3030 rpm gave the best exit edge because the last sheet was sheared rather than bent. Table 4 summarises the edge-quality metrics per drill and face.
3.6. Contribution Analysis and Multi-Objective Optimisation
The ANOVA of Table 3 used the unreplicated first series. The complete data set comprises three replicated series of the 3³ plan (81 measurements), which allows the full model, including the three-factor interaction, to be estimated with 54 error degrees of freedom. This section ranks the effects of drill type, speed and feed on five hole-quality criteria and then finds the best compromise by RSM [62,63] with a weighted desirability function [64] and exhaustive grid search; previous multi-criteria studies of FML drilling relied mainly on Taguchi-based grey relational analysis [46,51] and on RSM with ANOVA [54]. The five responses are Fmax, Tw, Tmax, BHout and BRout (Section 2.4). BHout is a non-contact, circumferentially averaged counterpart of the stylus-measured burr heights reported for GLARE and metals [32,34,66,96], so absolute values should not be compared directly with the literature; BRout, introduced here, quantifies the circumferential extent of the push-out of the bottom sheet. Because depressed edges are also defects, |BHout| is minimised in the optimisation, whereas the signed BHout is used in the contribution analysis (negative condition means occurred for carbide at 715 rpm/0.2 mm/rev and 3030 rpm/0.1 mm/rev and for HSS-R at 3030 rpm/0.3 mm/rev).
3.6.1. Contribution Analysis
The contribution of each term is its sum of squares as a percentage of the total over the 81 observations (Table 5; Figure S6). The full model explained 97.8–99.98% of the variation of the five responses and the replicate error only 0.02–2.24%. Because the error mean square is so small, almost every term is statistically significant, so the terms are ranked by their contributions.
Drill type dominated the thermo-mechanical responses. It contributed 51.9% to Fmax (speed 5.5%, feed 1.4%), with means of 33.8 N for HSS-G, 38.6 N for HSS-R and 41.8 N for the carbide drill, confirming the ranking of the 27-hole ANOVA. The order follows the chisel-edge geometry that carries most of the axial load: the carbide drill is 6% larger in diameter and less sharp, so a larger share of its thrust goes into ploughing, whereas the sharp, symmetrically ground lips and thin web of the HSS-G drill shear the 7075-T6 sheets and the glass/epoxy plies. Feed is unimportant because the chip thickness per lip (f/2 = 0.05–0.15 mm) is limited and the chisel edge engages one 0.41 mm sheet at a time; the 19.8% three-factor interaction reflects the chip-packing events of the HSS-G drill at 0.2 mm/rev (E9, E45; Fmax = 38.0 N versus 32.5 N in the other HSS-G conditions). Drill type also governed Tw (35.9%; 31.0, 28.8 and 27.0 °C for carbide, HSS-G and HSS-R), consistent with the correlation between Tw and thrust (r = 0.62), whereas speed (6.7%) and feed (3.6%) mattered little because of the short contact time (0.2–2.1 s); the isolated warm conditions behind the 25.7% three-factor term (33.8–35.4 °C) all remained far below the glass transition of the epoxy. Feed was the leading predictor of Tmax (45.6%; 102.3, 105.8 and 116.2 °C at 0.1, 0.2 and 0.3 mm/rev), speed acted non-monotonically (9.4%; 104.3, 110.2 and 109.7 °C at 715, 1520 and 3030 rpm) through the competition between heat generation and drilling time, which also explains the 13.2% speed × feed interaction, and drill type was minor (2.6%; 107.8, 106.5 and 109.9 °C for HSS-R, HSS-G and carbide).
The edge responses behaved differently: the main effects explained only 12.8% of the variance of BHout, the two-factor interactions 52.9% (drill × speed 24.9%, drill × feed 23.1%) and the three-factor interaction 34.3%. Burr height therefore cannot be controlled by speed or feed alone; their effect depends on the drill. For the carbide drill the mean BHout was 14.5, 98.6 and 1.8 µm at 715, 1520 and 3030 rpm and 30.2, −0.8 and 85.5 µm at 0.1, 0.2 and 0.3 mm/rev, whereas the HSS drills stayed within 7–27 µm (HSS-R) and 12–24 µm (HSS-G, excluding E9) at all settings. The exit burr forms when the unsupported bottom sheet is displaced by the chisel edge and then sheared by the lips [21], and its type and size depend on the cutting conditions and the drill geometry [96]: if the axial load and strain rate cause shear failure the burr is small, whereas if the sheet yields under the lips a tall burr or a rolled edge results. The large-diameter carbide drill transfers the highest axial load through its chisel edge and displaces the sheet at 1520 rpm or 0.3 mm/rev, whereas at 3030 rpm the sheet is sheared before it can bend (Section 3.3); the smaller load and sharper lips of the HSS drills give a flat response. The bulging ratio followed the same pattern (main effects 28.1%, two-factor interactions 36.8%, three-factor interaction 35.0%), and the three-factor term is dominated by a single condition: the chip-clogged HSS-G condition at 715 rpm/0.2 mm/rev (condition means BHout = 239 µm, BRout = 83%) accounts for 49.8% and 59.9% of the total sums of squares of BHout and BRout. Replacing its three observations by the mean of the remaining conditions raised the drill-type contribution to BRout from 14.8% to 57.0% (57.8% in Table 3, where E9 was removed), reduced the three-factor term to 17.3% (BRout) and 16.6% (BHout) and raised the drill × speed term for BHout to 29.3%. Without E9 the carbide drill retains the highest bulging ratio (22.3% versus 6.1% for HSS-R and 3.7% for HSS-G), consistent with its larger axial load and the push-out mechanism, and the weight of a single clogging event confirms that chip evacuation can outweigh the nominal parameters.
3.6.2. Problem Formulation and Response-Surface Models
The decision variables are the drill type (HSS-R, HSS-G, carbide), the spindle speed n (715–3030 rpm, i.e. 13.5–57.1 m/min for the Ø6.00 mm drills and 14.3–60.4 m/min for the Ø6.35 mm carbide drill) and the feed f (0.10–0.30 mm/rev). Five responses are minimised simultaneously: Fmax, Tw, Tmax, |BHout| and BRout. Importance weights of 3 were assigned to the three thermo-mechanical responses and 5 to the two edge responses (Table 6), because the exit burr is the dominant defect of the 3-3/2 laminate (Section 3.3) and requires secondary removal. Each response yi was converted into a one-sided smaller-is-better desirability di [64] with the lower and upper limits Li and Ui equal to the minimum and maximum of the 81 measurements (Equation (1)), and the responses were combined into the weighted composite desirability D (Equation (2)):
where d1…d5 refer to Fmax, Tw, Tmax, |BHout| and BRout and the exponents are the weights (Σwi = 19). Because the geometric mean is zero when any response reaches its upper limit, a condition cannot score well by excelling in four responses while failing in the fifth. The weighted-sum score S [98] was computed as an independent cross-check (Equation (3)). The problem is to maximise D(drill, n, f) subject to 715 ≤ n ≤ 3030 rpm and 0.10 ≤ f ≤ 0.30 mm/rev.
di = 1 (yi ≤ Li); di = [(Ui − yi)/(Ui − Li)]s (Li < yi < Ui); di = 0 (yi ≥ Ui); s = 1 (1)
D = (d13 · d23 · d33 · d45 · d55)1/19 (2)
S = (3d1 + 3d2 + 3d3 + 5d4 + 5d5)/19 (3)
Because drill type is categorical, drill-wise second-order models (six coefficients from nine conditions per drill) were considered first, but leave-one-condition-out cross-validation, in which the three replicates of one condition are removed in turn, gave negative cross-validated R² for all five responses (−0.62 to −3.87), and they were discarded. The continuous variables were therefore coded according to Equation (4), with a logarithmic speed coding that places the step-pulley speeds 715, 1520 and 3030 rpm at x1 = −1, +0.04 and +1, and pooled second-order models with drill-specific intercepts were fitted (Equation (5)):
where DG and DC are indicator variables for the HSS-G and carbide drills (HSS-R is the reference level). The models were fitted by ordinary least squares to all 81 observations (8 coefficients, 73 residual degrees of freedom) with a lack-of-fit test based on the pure error of the replicates. Two grids were searched exhaustively: Grid A, the 27 machine-feasible conditions, evaluated with the measured condition means (n = 3), and Grid B, a refined grid of 3 drills × 464 speeds (715–3030 rpm, 5 rpm step) × 41 feeds (0.100–0.300 mm/rev, 0.005 mm/rev step), i.e. 57,072 RSM predictions with the edge responses clamped at zero. The complete set of control parameters and the workflow are given in Table S2 and Figure S7.
x1 = [ln n − ½(ln 715 + ln 3030)]/[½ ln(3030/715)], x2 = (f − 0.20)/0.10 (4)
y = β0 + βGDG + βCDC + β1x1 + β2x2 + β11x12 + β22x22 + β12x1x2 + ε (5)
3.6.3. Response-Surface Results
The pooled models describe the thermo-mechanical responses reasonably well (adjusted R² = 0.57 for Fmax, 0.41 for Tw and 0.66 for Tmax; cross-validated R² = 0.20, −0.07 and 0.37), whereas the edge-quality models explain only 16–22% of the variance and have negative cross-validated R² (−0.45 and −0.34); the lack-of-fit test was significant for all responses (p < 0.001) because the pure error of the replicates is extremely small (median CV 2.0% for Fmax and 2.8% for BHout). First-order models gave slightly higher cross-validated R² for Fmax and Tw (0.28 and 0.13) but a lower value for Tmax (0.25 versus 0.37), so the second-order form was retained; the full statistics are listed in Table S3. The coefficients (Table 7) confirm the contribution analysis: the carbide drill raises Fmax by 3.2 N and Tw by 4.0 °C, HSS-G lowers Fmax by 4.8 N relative to HSS-R (p < 0.001), the positive curvature of Fmax in speed (β11 = 2.20 N, p < 0.01) places its minimum at 1390 rpm, where the main-effect plot shows a shallow minimum, and Tmax depends on feed (β2 = 6.98 °C) and on the speed × feed interaction (β12 = −4.38 °C; both p < 0.001), which corresponds to the trade-off between heat input and drilling time. For the edge responses only the carbide intercept (+39.7 µm and +16.2%) and the negative linear speed term (−17.6 µm and −5.7% per coded unit) are significant, i.e. a higher speed reduces both burr height and bulging ratio, as in RSM studies of drilling burrs in aluminium-matrix composites [65,66].
The response surfaces and the measured condition means are shown in Figure 8. By construction the three drill surfaces are parallel and differ only in their intercepts (Table 7). The measured means scatter widely around the smooth edge-response surfaces (Figure 8d,e), most strongly at the isolated conditions with burr heights above 140 µm, in line with the low R² values: edge-defect formation is governed by condition-specific events rather than by a smooth function of speed and feed. The composite-desirability surfaces (Figure 8f; refined grid in Figure S8) peak at low feed and intermediate speed and are lower for the carbide drill than for the HSS drills.
3.6.4. Optimum Conditions
On the machine-feasible grid (Table 8; complete ranking in Table S1 and Figure S9) the highest desirability, D = 0.867, was obtained for the HSS-G drill at 1520 rpm and 0.2 mm/rev (Fmax = 31.1 N, Tw = 27.2 °C, Tmax = 102.5 °C, |BHout| = 1.8 µm, BRout = 0.8%), followed by HSS-G at 1520 rpm with 0.1 mm/rev (D = 0.852) and 0.3 mm/rev (D = 0.825). The three best conditions thus form a plateau of the ground HSS drill at the intermediate speed, irrespective of feed. The best condition has almost perfect edge desirabilities (1.00 and 0.99) but the lowest desirability of its five components for the drill temperature (0.59). Ranks four and five (carbide at 715 rpm/0.1 mm/rev and HSS-R at 715 rpm/0.2 mm/rev) combine low drill and workpiece temperatures (91.8 and 98.9 °C; 25.4 and 24.9 °C) with higher thrust (34.6 and 35.8 N) and sizeable burrs (|BHout| = 42 and 38 µm). The worst conditions are the chip-clogged HSS-G condition at 715 rpm/0.2 mm/rev (D = 0.027; |BHout| = 239 µm, BRout = 83%), carbide at 715 rpm/0.2 mm/rev (D = 0.241) and carbide at 1520 rpm/0.3 mm/rev (D = 0.235; Tmax = 127.4 °C, |BHout| = 148 µm). The weighted-sum score gave almost the same ranking (Spearman ρ = 0.98; identical top five).
The refined RSM search over 57,072 candidates selected the HSS-R drill at 1325 rpm and the minimum feed of 0.100 mm/rev (D = 0.814); the best HSS-G candidate (1295 rpm, 0.100 mm/rev; D = 0.809) is almost equal and the best carbide candidate much lower (1390 rpm, 0.100 mm/rev; D = 0.624). The predicted responses at the HSS-R optimum are Fmax = 36.7 ± 1.8 N, Tw = 25.5 ± 1.2 °C, Tmax = 102.9 ± 3.0 °C, |BHout| = 17.7 ± 26.3 µm and BRout = 1.0 ± 9.0% (95% confidence intervals of the mean; Table S4). The two optimisations agree on the HSS drills and on the central speed range (1300–1520 rpm) but differ in the choice between HSS-R and HSS-G and in the feed (0.10 versus 0.20 mm/rev); the difference in objective value is small, since HSS-G at 1520 rpm/0.1 mm/rev (D = 0.852) lies only 0.015 below the measured optimum. The RSM reproduces the responses of the tested condition nearest to its optimum (HSS-R, 1520 rpm, 0.1 mm/rev) for Tmax, |BHout| and BRout but underestimates Fmax (36.5 versus 39.1 N) and Tw (25.6 versus 27.4 °C), and it fails for the best measured condition, predicting |BHout| = 54.6 ± 26.4 µm and BRout = 16.2 ± 9.0% where 1.8 µm and 0.8% were measured and ranking it eighth of 27 (Table S4). Across the 27 conditions the Spearman correlation between predicted and measured D is 0.71 (p < 0.001): the RSM captures the general pattern of the objective but not its detailed ranking, and because its optimum lies on the feed boundary it cannot locate an interior optimum. The recommendation is therefore based on the measured grid, with the RSM providing the trends of Table 7 and confirming the region around the central speed.
3.6.5. Sensitivity and Robustness
Table 9 shows the effect of the weighting. The measured optimum (HSS-G, 1520 rpm, 0.2 mm/rev) is retained with equal weights (S2) and with edge-dominated weights (S3, S5), and it is replaced by carbide at 715 rpm/0.1 mm/rev (D = 0.816) only when the thermo-mechanical responses are weighted five times more than the edge responses (S4), where its low drill and workpiece temperatures outweigh the burr. The RSM optimum is less stable in drill type and speed (HSS-R or HSS-G at 945–2595 rpm) but always lies on the lower feed boundary, again revealing the weakness of the edge models. In a stratified bootstrap [97] (1000 resamples of the replicates within each condition) HSS-G/1520 rpm/0.2 mm/rev ranked first in every resample, and the refitted RSM selected HSS-R at about 1325 rpm and 0.1 mm/rev in 98.9% of the resamples (HSS-G at about 1285 rpm in 1.1%; standard deviation of the speed 24 rpm). This stability should not be over-interpreted, because the resampling reflects only the variation between the three replicates of each condition and not the hole-to-hole, sheet-to-sheet and tool-to-tool variation of a confirmation experiment.
3.7. Practical Recommendations and Limitations
The hole-by-hole results (Section 3.1, Section 3.2, Section 3.3, Section 3.4 and Section 3.5) and the replicated contribution analysis and optimisation (Section 3.6) lead to the following guidelines for dry drilling of GLARE 3-3/2 on conventional machine tools. (1) The ground HSS drill is the most balanced choice: it produced the lowest thrust, nominal-size holes at both faces, the flattest entry edges and small, reproducible exit burrs, and it occupies the first three ranks of the desirability optimisation. At 1520 rpm (28.7 m/min) a feed of 0.2 mm/rev gives the highest desirability (D = 0.867) and twice the feed velocity of 0.1 mm/rev (304 versus 152 mm/min), which is an almost equal alternative (D = 0.852). Its only failure mode was chip packing at 0.2 mm/rev and the two extreme speeds (E9, E45), which peck drilling or chip-evacuation monitoring can prevent. (2) The rolled HSS drill is not recommended where the entry-diameter tolerance or the hole integrity matters, because it produces a 0.2–0.5 mm bell mouth and promotes fibre pull-out, matrix chipping and local interface debonding; if it is used, 3030 rpm reduces both entry roll-over and exit burr. (3) The carbide-tipped drill gives the most accurate and roundest holes and the cleanest walls, but it must be run at 3030 rpm and ≤0.2 mm/rev to avoid 60–150 µm exit burrs at 1520 rpm or 0.3 mm/rev; because of its higher thrust and workpiece temperature it is overall less desirable than the HSS drills unless the thermo-mechanical responses are weighted much more heavily than the edge responses (scenario S4). (4) The feed should not exceed 0.2 mm/rev with HSS drills, since the drill temperature exceeded 110 °C at 0.3 mm/rev for all drills. In summary, drill type sets the thermo-mechanical load (52% of Fmax, 36% of Tw), feed sets the drill temperature (46%) and the edge quality depends on the drill-specific speed–feed combination. These recommendations for thin 3-3/2 laminates are consistent with the findings of Giasin et al. [34,35] and Park et al. [44] for thicker GLARE grades.
Several limitations apply. (a) The hole-by-hole ANOVA (Table 3) used a single series with the three-factor interaction as the error term and therefore had little power for small effects, and each face was scanned once. (b) The edge responses do not follow smooth response surfaces, so the recommended condition rests on direct measurement and on its stability across the weight scenarios rather than on the model. (c) The desirability limits were taken from the observed ranges, which the single chip-clogged hole widened for the edge responses; 21 of the 27 conditions therefore have a |BHout| desirability above 0.8 (20 for BRout), which compresses the differences between acceptable conditions. (d) Chip packing occurred for HSS-G at 0.2 mm/rev at both extreme speeds, and the recommended condition lies between them, so its freedom from chip packing must be confirmed. (e) The replicate scatter is very small (error 0.02–0.03% of the variation of BHout and BRout; maximum replicate range of BHout 4.4 µm), far smaller than the usual hole-to-hole variability of drilling burrs, so the contributions of Table 5 and the bootstrap reflect the repeatability of the measurement chain, and a confirmation experiment with newly drilled holes is required. (f) The SEM study was qualitative, covered twelve of the 27 holes and excluded the HSS-G drill. (g) Torque and tool wear were not measured, and the optimum applies to the drill diameters, the 2.55 mm laminate and the bench drilling machine used. The aperture and edge-band metrics, however, are automatic and threshold-free and can be applied to any through-hole scan; their extension to CMM-verified diameters, coated drills and confirmation experiments is in progress.
4. Conclusions
Dry drilling of autoclave-cured GLARE 3-3/2 laminates with rolled HSS, ground HSS and carbide-tipped drills was studied in a 3³ full factorial design with thrust-force, infrared-temperature and profilometric measurements of every hole, SEM of the sectioned walls, contribution analysis of replicated data and RSM–desirability–grid-search optimisation. Drill type was the only significant factor for the thrust force (29.6% contribution; 33.3 N for HSS-G, 36.9 N for HSS-R and 39.5 N for carbide), whereas feed governed the maximum drill temperature (101.5–114.6 °C from 0.1 to 0.3 mm/rev) irrespective of drill type, and the workpiece temperature stayed below 43 °C.
Exit burrs, not entry damage, were the dominant edge defect (mean burr height −3.9 µm at entry versus +25.7 µm at exit; p < 0.001). The ground HSS drill produced holes closest to the nominal size (within ±0.04 mm), the flattest entry faces and the smallest exit bulging ratio (3.7%); the rolled HSS drill produced bell-mouthed entries (+0.30 ± 0.17 mm) and the most entry roll-over; the carbide drill produced the most accurate holes but the largest exit burrs (up to 152 µm) at 1520 rpm or 0.3 mm/rev, which vanished at 3030 rpm. A single chip-clogging event of the ground HSS drill produced a 245 µm burr, showing that chip evacuation can override the nominal parameters. SEM showed that the rolled HSS drill removes the glass plies by fibre pull-out and damages the adhesive interlayers by matrix chipping, aluminium smearing and debonding, whereas the carbide drill shears the fibres transversely and leaves continuous walls with local aluminium smearing and fibre crushing; the ranking of the two drills therefore reverses between the hole face and the hole wall.
In the replicated data set (81 holes) drill type contributed 52% of the variation of Fmax and 36% of Tw, feed contributed 46% of Tmax, and two- and three-factor interactions explained 72–87% of the variation of BHout and BRout. The ground HSS drill at 1520 rpm and 0.2 mm/rev was the best compromise (D = 0.867; Fmax = 31.1 N, Tmax = 102.5 °C, |BHout| = 1.8 µm, BRout = 0.8%) and remained so under alternative weightings and bootstrap resampling. Because the RSM described only the thermo-mechanical responses, the recommendation is based on the measured grid.
For burr-free, dimensionally accurate dry drilling of GLARE 3-3/2 on conventional machines, a ground HSS drill at 1520 rpm and 0.1–0.2 mm/rev with chip control is recommended, or a carbide-tipped drill at 3030 rpm and ≤0.2 mm/rev where dimensional accuracy has priority; rolled HSS drills should be avoided where the entry-diameter tolerance matters. A confirmation experiment is required before the optimum is transferred to production.
Supplementary Materials
The following supporting information can be downloaded at the website of this paper posted on Preprints.org. Supplementary Note S1: infrared thermograms at drill withdrawal; Supplementary Note S2: instrument-reported hole and peak areas; Figure S1: main-effect plots of the mean thrust force and the maximum drill temperature; Figure S2: infrared thermograms at drill withdrawal; Figure S3: aperture oversize and out-of-roundness; Figure S4: instrument-reported hole and peak areas; Figure S5: exit burr height and bulging ratio versus thrust force and drill temperature; Figure S6: contributions of the model terms to the total sum of squares; Figure S7: workflow of the contribution analysis and optimisation; Figure S8: composite desirability over the refined grid; Figure S9: ranked composite desirability of the 27 conditions and individual desirabilities; Table S1: condition means, composite desirability and rank of the 27 conditions; Table S2: control parameters of the RSM–desirability–grid-search optimisation; Table S3: statistics of the pooled second-order RSM models; Table S4: measured and RSM-predicted responses at the measured and RSM optima.
Author Contributions
Conceptualization, S.F. and S.Ü.; methodology, S.F.; investigation, Ç.Ç.; resources, M.Ö.B. and E.Y.; data curation, Ç.Ç. and S.Ü.; formal analysis, S.F.; validation, M.İ.Ö. and E.Y.; visualization, S.F.; writing—original draft preparation, Ç.Ç. and S.F.; writing—review and editing, S.Ü., M.Ö.B., M.İ.Ö., E.Y. and S.F.; supervision, S.F. All authors have read and agreed to the published version of the manuscript.
Funding
This research received no external funding.
Institutional Review Board Statement
Not applicable.
Data Availability Statement
The thrust-force, temperature and profilometric data supporting the findings of this study are available from the corresponding author upon reasonable request.
Acknowledgments
The authors thank the Kocaeli University Wear Laboratory for the profilometric measurements.
Conflicts of Interest
The authors declare no conflict of interest.
References
- Sinmazçelik, T.; Avcu, E.; Bora, M.Ö.; Çoban, O. A review: Fibre metal laminates, background, bonding types and applied test methods. Mater. Des. 2011, 32, 3671–3685. [Google Scholar] [CrossRef]
- Vermeeren, C.A.J.R. An Historic Overview of the Development of Fibre Metal Laminates. Appl. Compos. Mater. 2003, 10, 189–205. [Google Scholar] [CrossRef]
- Vogelesang, L.B.; Vlot, A. Development of fibre metal laminates for advanced aerospace structures. J. Mater. Process. Technol. 2000, 103, 1–5. [Google Scholar] [CrossRef]
- Gunnink, J.W.; Vlot, A.; de Vries, T.J.; van der Hoeven, W. Glare Technology Development 1997–2000. Appl. Compos. Mater. 2002, 9, 201–219. [Google Scholar] [CrossRef]
- Vlot, A.; Gunnink, J.W. (Eds.) Fibre Metal Laminates; Kluwer Academic Publishers: Dordrecht, The Netherlands, 2001. [Google Scholar] [CrossRef]
- Alderliesten, R.C.; Hagenbeek, M.; Homan, J.J.; Hooijmeijer, P.A.; de Vries, T.J.; Vermeeren, C.A.J.R. Fatigue and Damage Tolerance of Glare. Appl. Compos. Mater. 2003, 10, 223–242. [Google Scholar] [CrossRef]
- Wu, G.; Yang, J.-M. The mechanical behavior of GLARE laminates for aircraft structures. JOM 2005, 57, 72–79. [Google Scholar] [CrossRef]
- Asundi, A.; Choi, A.Y.N. Fiber metal laminates: An advanced material for future aircraft. J. Mater. Process. Technol. 1997, 63, 384–394. [Google Scholar] [CrossRef]
- Sinke, J. Manufacturing of GLARE Parts and Structures. Appl. Compos. Mater. 2003, 10, 293–305. [Google Scholar] [CrossRef]
- Caggiano, M.; Saffioti, M.R.; Rotella, G. Fiber Metal Laminates: The Role of the Metal Surface and Sustainability Aspects. J. Compos. Sci. 2025, 9, 35. [Google Scholar] [CrossRef]
- Costa, R.D.F.S.; Sales-Contini, R.C.M.; Silva, F.J.G.; Sebbe, N.; Jesus, A.M.P. A Critical Review on Fiber Metal Laminates (FML): From Manufacturing to Sustainable Processing. Metals 2023, 13, 638. [Google Scholar] [CrossRef]
- Franz, G.; Vantomme, P.; Hassan, M.H. A Review on Drilling of Multilayer Fiber-Reinforced Polymer Composites and Aluminum Stacks: Optimization of Strategies for Improving the Drilling Performance of Aerospace Assemblies. Fibers 2022, 10, 78. [Google Scholar] [CrossRef]
- Slamani, M.; Chatelain, J.-F. A review on the machining of polymer composites reinforced with carbon (CFRP), glass (GFRP), and natural fibers (NFRP). Discov. Mech. Eng. 2023, 2. [Google Scholar] [CrossRef]
- Rahme, P. A bibliometric analysis on drilling of composite materials using a systematic approach. Heliyon 2024, 10, e37282. [Google Scholar] [CrossRef]
- Jagadeesh, P.; Mavinkere Rangappa, S.; Suyambulingam, I.; Siengchin, S.; Puttegowda, M.; Binoj, J.S.; Gorbatyuk, S.; Khan, A.; Doddamani, M.; Fiore, V.; Cuadrado, M.M.M. Drilling characteristics and properties analysis of fiber reinforced polymer composites: A comprehensive review. Heliyon 2023, 9, e14428. [Google Scholar] [CrossRef]
- Gao, T.; Zhang, Y.; Li, C.; Wang, Y.; Chen, Y.; An, Q.; Zhang, S.; Li, H.N.; Cao, H.; Ali, H.M.; Zhou, Z.; Sharma, S. Fiber-reinforced composites in milling and grinding: machining bottlenecks and advanced strategies. Front. Mech. Eng. 2022, 17. [Google Scholar] [CrossRef]
- Geier, N.; Davim, J.P.; Szalay, T. Advanced cutting tools and technologies for drilling carbon fibre reinforced polymer (CFRP) composites: A review. Compos. Part A Appl. Sci. Manuf. 2019, 125, 105552. [Google Scholar] [CrossRef]
- Shetty, N.; Shahabaz, S.M.; Sharma, S.S.; Shetty, S.D. A review on finite element method for machining of composite materials. Compos. Struct. 2017, 176, 790–802. [Google Scholar] [CrossRef]
- Pramanik, A.; Basak, A.K.; Dong, Y.; Sarker, P.K.; Uddin, M.S.; Littlefair, G.; Dixit, A.R.; Chattopadhyaya, S. Joining of carbon fibre reinforced polymer (CFRP) composites and aluminium alloys – A review. Compos. Part A Appl. Sci. Manuf. 2017, 101, 1–29. [Google Scholar] [CrossRef]
- Ürgün, S.; Fidan, S.; Yarar, E.; Özsoy, M.İ.; Bora, M.Ö. Effect of stacking sequence and drilling parameters on the thermomechanical response of carbon/glass fiber reinforced epoxy composites using a novel HSS flow step drill; Polymers, 2026. [Google Scholar]
- Hocheng, H.; Dharan, C.K.H. Delamination During Drilling in Composite Laminates. J. Eng. Ind. 1990, 112, 236–239. [Google Scholar] [CrossRef]
- Jain, S.; Yang, D.C.H. Effects of Feedrate and Chisel Edge on Delamination in Composites Drilling. J. Eng. Ind. 1993, 115, 398–405. [Google Scholar] [CrossRef]
- Chen, W.-C. Some experimental investigations in the drilling of carbon fiber-reinforced plastic (CFRP) composite laminates. Int. J. Mach. Tools Manuf. 1997, 37, 1097–1108. [Google Scholar] [CrossRef]
- Hocheng, H.; Tsao, C.C. Comprehensive analysis of delamination in drilling of composite materials with various drill bits. J. Mater. Process. Technol. 2003, 140, 335–339. [Google Scholar] [CrossRef]
- Hocheng, H.; Tsao, C.C. Effects of special drill bits on drilling-induced delamination of composite materials. Int. J. Mach. Tools Manuf. 2006, 46, 1403–1416. [Google Scholar] [CrossRef]
- Davim, J.; Rubio, J.; Abrao, A. A novel approach based on digital image analysis to evaluate the delamination factor after drilling composite laminates. Compos. Sci. Technol. 2007, 67, 1939–1945. [Google Scholar] [CrossRef]
- Silva, D.; Pamies Teixeira, J.; Machado, C.M. Methodology analysis for evaluation of drilling-induced damage in composites. Int. J. Adv. Manuf. Technol. 2014, 71, 1919–1928. [Google Scholar] [CrossRef]
- Babu, J.; Sunny, T.; Paul, N.A.; Mohan, K.P.; Philip, J.; Davim, J.P. Assessment of delamination in composite materials: A review. Proc. Inst. Mech. Eng. Part B J. Eng. Manuf. 2016, 230, 1990–2003. [Google Scholar] [CrossRef]
- Geng, D.; Liu, Y.; Shao, Z.; Lu, Z.; Cai, J.; Li, X.; Jiang, X.; Zhang, D. Delamination formation, evaluation and suppression during drilling of composite laminates: A review. Compos. Struct. 2019, 216, 168–186. [Google Scholar] [CrossRef]
- Qiu, X.; Li, P.; Li, C.; Niu, Q.; Chen, A.; Ouyang, P.; Ko, T.J. Study on chisel edge drilling behavior and step drill structure on delamination in drilling CFRP. Compos. Struct. 2018, 203, 404–413. [Google Scholar] [CrossRef]
- Giasin, K.; Ayvar-Soberanis, S.; Hodzic, A. An experimental study on drilling of unidirectional GLARE fibre metal laminates. Compos. Struct. 2015, 133, 794–808. [Google Scholar] [CrossRef]
- Giasin, K.; Ayvar-Soberanis, S. An Investigation of burrs, chip formation, hole size, circularity and delamination during drilling operation of GLARE using ANOVA. Compos. Struct. 2017, 159, 745–760. [Google Scholar] [CrossRef]
- Giasin, K.; Ayvar-Soberanis, S.; French, T.; Phadnis, V. 3D Finite Element Modelling of Cutting Forces in Drilling Fibre Metal Laminates and Experimental Hole Quality Analysis. Appl. Compos. Mater. 2017, 24, 113–137. [Google Scholar] [CrossRef]
- Giasin, K.; Gorey, G.; Byrne, C.; Sinke, J.; Brousseau, E. Effect of machining parameters and cutting tool coating on hole quality in dry drilling of fibre metal laminates. Compos. Struct. 2019, 212, 159–174. [Google Scholar] [CrossRef]
- Giasin, K.; Hawxwell, J.; Sinke, J.; Dhakal, H.; Köklü, U.; Brousseau, E. The effect of cutting tool coating on the form and dimensional errors of machined holes in GLARE® fibre metal laminates. Int. J. Adv. Manuf. Technol. 2020, 107, 2817–2832. [Google Scholar] [CrossRef]
- Giasin, K.; Dad, A.; Brousseau, E.; Pimenov, D.; Mia, M.; Morkavuk, S.; Koklu, U. The effects of through tool cryogenic machining on the hole quality in GLARE® fibre metal laminates. J. Manuf. Process. 2021, 64, 996–1012. [Google Scholar] [CrossRef]
- Giasin, K.; Ayvar-Soberanis, S.; Hodzic, A. Evaluation of cryogenic cooling and minimum quantity lubrication effects on machining GLARE laminates using design of experiments. J. Clean. Prod. 2016, 135, 533–548. [Google Scholar] [CrossRef]
- Giasin, K.; Atif, M.; Ma, Y.; Jiang, C.; Koklu, U.; Sinke, J. Machining GLARE fibre metal laminates: a comparative study on drilling effect between conventional and ultrasonic-assisted drilling. Int. J. Adv. Manuf. Technol. 2022, 123, 3657–3672. [Google Scholar] [CrossRef]
- Pawar, O.A.; Gaikhe, Y.S.; Tewari, A.; Sundaram, R.; Joshi, S.S. Analysis of hole quality in drilling GLARE fiber metal laminates. Compos. Struct. 2015, 123, 350–365. [Google Scholar] [CrossRef]
- Akula, S.; Bolar, G. Comparative evaluation of machining processes for making holes in GLARE fiber metal laminates. Mater. Today Proc. 2021, 46, 9126–9131. [Google Scholar] [CrossRef]
- Tyczyński, P.; Lemańczyk, J.; Ostrowski, R.; Śliwa, R.E. Drilling of CFRP, GFRP, glare type composites. Aircr. Eng. Aerosp. Technol. 2014, 86, 312–322. [Google Scholar] [CrossRef]
- Sorrentino, L.; Turchetta, S.; Parodo, G. Drilling of glare laminates: effect of cutting parameters on process forces and temperatures. Int. J. Adv. Manuf. Technol. 2022, 120, 645–657. [Google Scholar] [CrossRef]
- Boughdiri, I.; Giasin, K.; Mabrouki, T.; Zitoune, R. Effect of cutting parameters on thrust force, torque, hole quality and dust generation during drilling of GLARE 2B laminates. Compos. Struct. 2021, 261, 113562. [Google Scholar] [CrossRef]
- Park, S.Y.; Choi, W.J.; Choi, C.H.; Choi, H.S. Effect of drilling parameters on hole quality and delamination of hybrid GLARE laminate. Compos. Struct. 2018, 185, 684–698. [Google Scholar] [CrossRef]
- Ekici, E.; Motorcu, A.R.; Yıldırım, E. An experimental study on hole quality and different delamination approaches in the drilling of CARALL, a new FML composite. FME Trans. 2021, 49, 950–961. [Google Scholar] [CrossRef]
- Ekici, E.; Motorcu, A.R.; Uzun, G. Multi-objective optimization of process parameters for drilling fibermetal laminate using a hybrid GRA-PCA approach. FME Trans. 2021, 49, 356–366. [Google Scholar] [CrossRef]
- Ekici, E.; Pazarkaya, İ.; Uzun, G. Delamination and thrust force analysis in GLARE: Influence of tool geometry and prediction with machine learning models. J. Compos. Mater. 2025, 59, 1233–1249. [Google Scholar] [CrossRef]
- Mohan, N.; Kalam, S.A.; Mahaveerakannan, R.; Shah, M.; Yadav, J.S.; Sharma, V.; Naik, P.S.; Bharathi Narasimha, D. Statistical Evaluation of Machining Parameters in Drilling of Glass Laminate Aluminum Reinforced Epoxy Composites using Machine Learning Model. Eng. Sci. 2022, 20, 244–251. [Google Scholar] [CrossRef]
- Atif, M.; Wang, X.; Xie, L.; Sun, T.; Giasin, K.; Ma, Y. Influence of cutting tool design on ultrasonic-assisted drilling of fiber metal laminates. Int. J. Adv. Manuf. Technol. 2024, 131, 6039–6059. [Google Scholar] [CrossRef]
- Atif, M.; Wang, X.; Xie, L.; Giasin, K.; Ma, Y.; Jiang, C.; Koklu, U.; Sinke, J. Multiscale modelling and experimental analysis of ultrasonic-assisted drilling of GLARE fibre metal laminates. Compos. Part A Appl. Sci. Manuf. 2024, 177, 107962. [Google Scholar] [CrossRef]
- Logesh, K.; Moshi, A.A.M.; Bharathi, S.R.S.; Hariharasakthisudhan, P. A multi-objective grey relational approach and regression analysis on optimization of drilling process parameters for GLARE fiber metal laminates. Surf. Rev. Lett. 2022, 29, 2250066. [Google Scholar] [CrossRef]
- Bolar, G.; Dinesh, A.A.; Polishetty, A.; Shetty, R.; Hiremath, A.; Neelakantha, V.L. Performance Analysis of Helical Milling and Drilling Operations While Machining Carbon Fiber-Reinforced Aluminum Laminates. J. Manuf. Mater. Process. 2024, 8, 113. [Google Scholar] [CrossRef]
- Sourd, X.; Giasin, K.; Zitoune, R.; Salem, M.; Lupton, C. Multi-scale analysis of the damage and contamination in abrasive water jet drilling of GLARE fibre metal laminates. J. Manuf. Process. 2022, 84, 610–621. [Google Scholar] [CrossRef]
- Reddy, V.N.; Venkatesh, B. Optimization of parameters in abrasive water jet machining of glass laminate aluminium reinforced epoxy (GLARE). Mater. Today Proc. 2019, 19, 890–894. [Google Scholar] [CrossRef]
- Hariharasakthisudhan, P.; Logesh, K.; Kannan, S.; Sivakumar, R.; Sathickbasha, K. Optimizing the process parameter of abrasive water jet machining against sub-surface delamination of nanoclay modified GLARE laminates. Surf. Rev. Lett. 2024, 2550086. [Google Scholar] [CrossRef]
- Giasin, K.; Ayvar-Soberanis, S. Evaluation of Workpiece Temperature during Drilling of GLARE Fiber Metal Laminates Using Infrared Techniques: Effect of Cutting Parameters, Fiber Orientation and Spray Mist Application. Materials 2016, 9, 622. [Google Scholar] [CrossRef]
- Leonidas, E.; Ayvar-Soberanis, S.; Laalej, H.; Fitzpatrick, S.; Willmott, J.R. A Comparative Review of Thermocouple and Infrared Radiation Temperature Measurement Methods during the Machining of Metals. Sensors 2022, 22, 4693. [Google Scholar] [CrossRef]
- Merino-Pérez, J.L.; Royer, R.; Ayvar-Soberanis, S.; Merson, E.; Hodzic, A. On the temperatures developed in CFRP drilling using uncoated WC-Co tools Part I: Workpiece constituents, cutting speed and heat dissipation. Compos. Struct. 2015, 123, 161–168. [Google Scholar] [CrossRef]
- Merino-Pérez, J.L.; Hodzic, A.; Merson, E.; Ayvar-Soberanis, S. On the temperatures developed in CFRP drilling using uncoated WC-Co tools Part II: Nanomechanical study of thermally aged CFRP composites. Compos. Struct. 2015, 123, 30–34. [Google Scholar] [CrossRef]
- Fu, R.; Jia, Z.; Wang, F.; Jin, Y.; Sun, D.; Yang, L.; Cheng, D. Drill-exit temperature characteristics in drilling of UD and MD CFRP composites based on infrared thermography. Int. J. Mach. Tools Manuf. 2018, 135, 24–37. [Google Scholar] [CrossRef]
- Wang, F.-J.; Yin, J.-W.; Ma, J.-W.; Niu, B. Heat partition in dry orthogonal cutting of unidirectional CFRP composite laminates. Compos. Struct. 2018, 197, 28–38. [Google Scholar] [CrossRef]
- Box, G.E.P.; Wilson, K.B. On the Experimental Attainment of Optimum Conditions. J. R. Stat. Soc. Ser. B (Methodological) 1951, 13, 1–38. [Google Scholar] [CrossRef]
- Myers, R.H.; Montgomery, D.C.; Anderson-Cook, C.M. Response Surface Methodology: Process and Product Optimization Using Designed Experiments, 4th ed.; Wiley: Hoboken, NJ, USA, 2016; ISBN 978-1-118-91601-8. [Google Scholar]
- Derringer, G.; Suich, R. Simultaneous Optimization of Several Response Variables. J. Qual. Technol. 1980, 12, 214–219. [Google Scholar] [CrossRef]
- Thakre, A.A.; Soni, S. Modeling of burr size in drilling of aluminum silicon carbide composites using response surface methodology. Eng. Sci. Technol. An. Int. J. 2016, 19, 1199–1205. [Google Scholar] [CrossRef]
- Shanmughasundaram, P.; Subramanian, R. Study of parametric optimization of burr formation in step drilling of eutectic Al–Si alloy–Gr composites. J. Mater. Res. Technol. 2014, 3, 150–157. [Google Scholar] [CrossRef]
- Kilickap, E. Optimization of cutting parameters on delamination based on Taguchi method during drilling of GFRP composite. Expert Syst. With Appl. 2010, 37, 6116–6122. [Google Scholar] [CrossRef]
- Davim, J.P.; Reis, P. Study of delamination in drilling carbon fiber reinforced plastics (CFRP) using design experiments. Compos. Struct. 2003, 59, 481–487. [Google Scholar] [CrossRef]
- Ünüvar, A.; Öztürk, O. Machinability analysis of delamination and thrust force in drilling of pure and added GFRP composites. J. Compos. Mater. 2022, 57, 3–21. [Google Scholar] [CrossRef]
- Arul, S.; Samuel Raj, D.; Vijayaraghavan, L.; Malhotra, S.K.; Krishnamurthy, R. Modeling and Optimization of Process Parameters for Defect Toleranced Drilling of GFRP Composites. Mater. Manuf. Process. 2006, 21, 357–365. [Google Scholar] [CrossRef]
- Verma, R.K.; Pal, P.K.; Kandpal, B.C. Machining performance optimization in drilling of GFRP composites: A utility theory (UT) based approach. In Proceedings of the 2016 International Conference on Control, Computing, Communication and Materials (ICCCCM), Allahabad, India, 21–22 October 2016; IEEE; 2016, pp. 1–5. [Google Scholar] [CrossRef]
- Wang, Q.; Jia, X. Optimization of cutting parameters for improving exit delamination, surface roughness, and production rate in drilling of CFRP composites. Int. J. Adv. Manuf. Technol. 2021, 117, 3487–3502. [Google Scholar] [CrossRef]
- Kiliçkap, E.; Yardimeden, A.; Çelik, Y.H. Investigation of experimental study of end milling of CFRP composite. Sci. Eng. Compos. Mater. 2015, 22, 89–95. [Google Scholar] [CrossRef]
- Pascual, V.; San-Juan, M.; Santos, F.J.; Martín, Ó.; de Tiedra, M.P. Study of axial cutting forces and delamination phenomenon in drilling of carbon fiber composites. Procedia Manuf. 2017, 13, 67–72. [Google Scholar] [CrossRef]
- Kumar, J.; Verma, R.K. Delamination assessment during machining of laminated polymer nanocomposite. Int. J. Mod. Manuf. Technol. 2021, 13, 109–115. [Google Scholar] [CrossRef]
- Nikam, M.; Al-Lohedan, H.A.; Mohammad, F.; Khetree, S.; Patil, V.; Lonare, G.; Khan, F.J.; Jagatap, G.; Giri, J.P.; Oza, A.D.; Kumar, M.; Chadge, R.B.; Soleiman, A.A. Optimization of Machining Parameters for Enhanced Performance of Glass-Fibre-Reinforced Plastic (GFRP) Composites Using Design of Experiments. Sustainability 2023, 15, 12372. [Google Scholar] [CrossRef]
- Jenarthanan, M.P.; Nishanth, G.; Bharathwaj, R. Optimization of machining parameters in end milling of GFRP composites based on the Taguchi method with fuzzy logics. Int. J. Knowl.-Based Intell. Eng. Syst. 2016, 20, 123–134. [Google Scholar] [CrossRef]
- Jenarthanan, M.P.; Jeyapaul, R. Optimisation of machining parameters on milling of GFRP composites by desirability function analysis using Taguchi method. Int. J. Eng. Sci. Technol. 2018, 5, 22–36. [Google Scholar] [CrossRef]
- Palanikumar, K.; Karunamoorthy, L.; Karthikeyan, R. Multiple Performance Optimization of Machining Parameters on the Machining of GFRP Composites Using Carbide (K10) Tool. Mater. Manuf. Process. 2006, 21, 846–852. [Google Scholar] [CrossRef]
- Hussain, S.A.; Pandurangadu, V.; Kumar, K.P. Machining parameters optimisation in turning of GFRP composites by desirability function analysis embedded with Taguchi method. Int. J. Mach. Mach. Mater. 2015, 17, 95. [Google Scholar] [CrossRef]
- Bahei El-Deen, A. Multi optimization in slot milling of CFRP composites through grey relational-based Taguchi analysis. Niger. J. Technol. Dev. 2024, 21, 11–18. [Google Scholar] [CrossRef]
- Ducobu, F.; Mélice, E.; Rivière-Lorphèvre, E.; Beuscart, T.; Aizpuru, O.; Granjon, A.; Flores, P.; Soriano, D.; Cuesta, M.; Arrazola, P.-J. Sensitivity Analysis of Various Geometries of PCD and Cemented Tungsten Carbide Cutting Tools during the Milling of GFRP Composite. Polymers 2022, 14, 1524. [Google Scholar] [CrossRef]
- Raj, P.P.; Perumal, A.E. Taguchi Analysis of surface roughness and delamination associated with various cemented carbide K10 end mills in milling of GFRP. J. Eng. Sci. Technol. Rev. 2010, 3, 58–64. [Google Scholar] [CrossRef]
- Nurhaniza, M.; Ariffin, M.K.A.M.; Mustapha, F.; Baharudin, B.T.H.T. Analyzing the Effect of Machining Parameters Setting to the Surface Roughness during End Milling of CFRP-Aluminium Composite Laminates. Int. J. Manuf. Eng. 2016, 2016, 1–9. [Google Scholar] [CrossRef]
- Doluk, E.; Rudawska, A. Effect of Machining Settings and Tool Geometry on Surface Quality After Machining of Al/CFRP Sandwich Structures. Adv. Sci. Technol. Res. J. 2022, 16, 22–33. [Google Scholar] [CrossRef]
- Doluk, E.; Rudawska, A.; Miturska-Barańska, I. Investigation of the Surface Roughness and Surface Uniformity of a Hybrid Sandwich Structure after Machining. Materials 2022, 15, 7299. [Google Scholar] [CrossRef]
- Fernández-Pérez, J.; Cantero, J.L.; Díaz-Álvarez, J.; Miguélez, M.H. Hybrid Composite-Metal Stack Drilling with Different Minimum Quantity Lubrication Levels. Materials 2019, 12, 448. [Google Scholar] [CrossRef]
- Hamedanianpour, H.; Chatelain, J.F. Effect of Tool Wear on Quality of Carbon Fiber Reinforced Polymer Laminate during Edge Trimming. Appl. Mech. Mater. 2013, 325-326, 34–39. [Google Scholar] [CrossRef]
- Ozkan, D.; Panjan, P.; Gok, M.S.; Karaoglanli, A.C. Experimental Study on Tool Wear and Delamination in Milling CFRPs with TiAlN- and TiN-Coated Tools. Coatings 2020, 10, 623. [Google Scholar] [CrossRef]
- Sun, Z.; Geng, D.; Zheng, W.; Liu, Y.; Liu, L.; Ying, E.; Jiang, X.; Zhang, D. An innovative study on high-performance milling of carbon fiber reinforced plastic by combining ultrasonic vibration assistance and optimized tool structures. J. Mater. Res. Technol. 2023, 22, 2131–2146. [Google Scholar] [CrossRef]
- İç, Y.T.; Elaldı, F.; Keçeci, B.; Önder Uzun, G.; Limoncuoğlu, N.; Aksoy, İ. Kevlar fiber-epoksi kompozit malzemesinin frezeleme işleminin faktöriyel tasarım ve hedef programlama yöntemleriyle eniyilemesi (Optimization of milling parameters of Kevlar fiber–epoxy composite by factorial design and goal programming). Gazi Üniversitesi Mühendislik Mimar. Fakültesi Derg. 2019, 34, 1549–1560. [Google Scholar] [CrossRef]
- Alkhafaji, G.M.; Alshammaa, F.A.; Khalid, E.A. Fabricating Different Laminate Composites by Manual Layup and Estimating the Optimum Parameters for CNC Milling Machine. Al-Nahrain J. Eng. Sci. 2020, 23, 388–396. [Google Scholar] [CrossRef]
- Nguyen-Dinh, N.; Bouvet, C.; Zitoune, R. Influence of machining damage generated during trimming of CFRP composite on the compressive strength. J. Compos. Mater. 2020, 54, 1413–1430. [Google Scholar] [CrossRef]
- Hexcel Corporation. HexPly® BMS 8-139 Qualified Prepreg—Product Data Sheet; Hexcel: Stamford, CT, USA, 2020. [Google Scholar]
- Airbus Operations S.A.S. Structural Repair Manual (SRM), Chapter 53-15-12: Curing Parameters for GLARE Panels; Airbus: Blagnac, France, 2020. [Google Scholar]
- Kim, J.; Min, S.; Dornfeld, D.A. Optimization and control of drilling burr formation of AISI 304L and AISI 4118 based on drilling burr control charts. Int. J. Mach. Tools Manuf. 2001, 41, 923–936. [Google Scholar] [CrossRef]
- Efron, B.; Tibshirani, R.J. An Introduction to the Bootstrap; Chapman & Hall: New York, NY, USA, 1993. [Google Scholar] [CrossRef]
- Hwang, C.L.; Yoon, K. Multiple Attribute Decision Making: Methods and Applications. A State-of-the-Art Survey. In Lecture Notes in Economics and Mathematical Systems; Springer: Berlin/Heidelberg, Germany, 1981; Vol. 186. [Google Scholar] [CrossRef]
Figure 1.
(a) Mean and (b) maximum thrust force, (c) maximum drill temperature and (d) maximum chip temperature for the three drills at each spindle-speed/feed combination (first series, 27 holes; the 1520 rpm group is shaded).
Figure 1.
(a) Mean and (b) maximum thrust force, (c) maximum drill temperature and (d) maximum chip temperature for the three drills at each spindle-speed/feed combination (first series, 27 holes; the 1520 rpm group is shaded).

Figure 2.
Circumferentially averaged hole-edge height profiles at the entry face (upper half of each panel, plotted upward) and at the exit face (lower half, mirrored downward) for the HSS-R, HSS-G and carbide drills. Profiles are aligned at the hole wall (x = 0) and referenced to the undisturbed sheet surface; colour denotes spindle speed and line style denotes feed. The exit burr height of E9 (chip clogging, 245 µm) lies off-scale.
Figure 2.
Circumferentially averaged hole-edge height profiles at the entry face (upper half of each panel, plotted upward) and at the exit face (lower half, mirrored downward) for the HSS-R, HSS-G and carbide drills. Profiles are aligned at the hole wall (x = 0) and referenced to the undisturbed sheet surface; colour denotes spindle speed and line style denotes feed. The exit burr height of E9 (chip clogging, 245 µm) lies off-scale.

Figure 3.
(Top) Burr height adjacent to the hole wall at the entry face (BHin, blue) and at the exit face (BHout, orange); positive = raised burr, negative = rolled-over or chipped edge. (Bottom) Bulging ratio BR (percentage of the 0–300 µm edge band lying more than 40 µm above the reference plane, upward) and depressed fraction DF (more than 40 µm below, downward) at each face. Experiments are grouped by spindle speed (715/1520/3030 rpm; 1520 rpm shaded) with feed increasing 0.1 to 0.3 mm/rev within each group; off-scale values of E9 are annotated.
Figure 3.
(Top) Burr height adjacent to the hole wall at the entry face (BHin, blue) and at the exit face (BHout, orange); positive = raised burr, negative = rolled-over or chipped edge. (Bottom) Bulging ratio BR (percentage of the 0–300 µm edge band lying more than 40 µm above the reference plane, upward) and depressed fraction DF (more than 40 µm below, downward) at each face. Experiments are grouped by spindle speed (715/1520/3030 rpm; 1520 rpm shaded) with feed increasing 0.1 to 0.3 mm/rev within each group; off-scale values of E9 are annotated.

Figure 4.
Levelled height maps (10 × 10 mm) of the entry (top row) and exit (bottom row) faces for the HSS-R (E19), HSS-G (E21) and carbide (E23) drills at 1520 rpm/0.1 mm/rev, and for the chip-clogged HSS-G hole E9 (715 rpm/0.2 mm/rev). Colour scale ±100 µm; white = through-hole/non-measured.
Figure 4.
Levelled height maps (10 × 10 mm) of the entry (top row) and exit (bottom row) faces for the HSS-R (E19), HSS-G (E21) and carbide (E23) drills at 1520 rpm/0.1 mm/rev, and for the chip-clogged HSS-G hole E9 (715 rpm/0.2 mm/rev). Colour scale ±100 µm; white = through-hole/non-measured.

Figure 5.
Backscattered-electron SEM images (×20) of the sectioned hole walls for the HSS-R drill (a–f) and the carbide-tipped drill (g–l) at 715, 1520 and 3030 rpm (columns) and feeds of 0.1 and 0.3 mm/rev (rows); (g) was recorded in secondary-electron mode. Bright bands: 7075-T6 sheets; grey bands: glass/epoxy layers with the fabric ply in their centre. The face at the top of each panel is the exit sheet surface. Arrows mark the macroscopic wall defects discussed in the text. Scale bars 1 mm.
Figure 5.
Backscattered-electron SEM images (×20) of the sectioned hole walls for the HSS-R drill (a–f) and the carbide-tipped drill (g–l) at 715, 1520 and 3030 rpm (columns) and feeds of 0.1 and 0.3 mm/rev (rows); (g) was recorded in secondary-electron mode. Bright bands: 7075-T6 sheets; grey bands: glass/epoxy layers with the fabric ply in their centre. The face at the top of each panel is the exit sheet surface. Arrows mark the macroscopic wall defects discussed in the text. Scale bars 1 mm.

Figure 6.
Backscattered-electron SEM images (×100) of the hole walls drilled with the rolled HSS drill at (a) 715 rpm/0.1 mm/rev (E1), (b) 715 rpm/0.3 mm/rev (E13), (c) 1520 rpm/0.1 mm/rev (E19), (d) 1520 rpm/0.3 mm/rev (E31), (e) 3030 rpm/0.1 mm/rev (E37) and (f) 3030 rpm/0.3 mm/rev (E49). Arrows mark feed marks and ploughing of the aluminium sheets, fibre pull-out, crushed fibres and fibre fragments in the glass-fabric plies, smeared, chipped or torn-out matrix in the adhesive interlayers, pores of the adhesive film, an adhered aluminium chip fragment and interfacial debonding. Scale bars 100 µm.
Figure 6.
Backscattered-electron SEM images (×100) of the hole walls drilled with the rolled HSS drill at (a) 715 rpm/0.1 mm/rev (E1), (b) 715 rpm/0.3 mm/rev (E13), (c) 1520 rpm/0.1 mm/rev (E19), (d) 1520 rpm/0.3 mm/rev (E31), (e) 3030 rpm/0.1 mm/rev (E37) and (f) 3030 rpm/0.3 mm/rev (E49). Arrows mark feed marks and ploughing of the aluminium sheets, fibre pull-out, crushed fibres and fibre fragments in the glass-fabric plies, smeared, chipped or torn-out matrix in the adhesive interlayers, pores of the adhesive film, an adhered aluminium chip fragment and interfacial debonding. Scale bars 100 µm.

Figure 7.
Backscattered-electron SEM images (×100) of the hole walls drilled with the carbide-tipped drill at (a) 715 rpm/0.1 mm/rev (E5), (b) 715 rpm/0.3 mm/rev (E17), (c) 1520 rpm/0.1 mm/rev (E23), (d) 1520 rpm/0.3 mm/rev (E35), (e) 3030 rpm/0.1 mm/rev (E41) and (f) 3030 rpm/0.3 mm/rev (E53). Arrows mark the regular feed marks and the sharp sheet/composite interface, transversely sheared fibre ends, smeared resin, smeared or flaked aluminium, matrix flaking and cracking, crushed fibres, adhered debris and aluminium particles, the interface step and pores of the adhesive film. Scale bars 100 µm.
Figure 7.
Backscattered-electron SEM images (×100) of the hole walls drilled with the carbide-tipped drill at (a) 715 rpm/0.1 mm/rev (E5), (b) 715 rpm/0.3 mm/rev (E17), (c) 1520 rpm/0.1 mm/rev (E23), (d) 1520 rpm/0.3 mm/rev (E35), (e) 3030 rpm/0.1 mm/rev (E41) and (f) 3030 rpm/0.3 mm/rev (E53). Arrows mark the regular feed marks and the sharp sheet/composite interface, transversely sheared fibre ends, smeared resin, smeared or flaked aluminium, matrix flaking and cracking, crushed fibres, adhered debris and aluminium particles, the interface step and pores of the adhesive film. Scale bars 100 µm.

Figure 8.
RSM surfaces of (a) Fmax, (b) Tw, (c) Tmax, (d) |BHout|, (e) BRout and (f) composite desirability D as functions of spindle speed and feed for the three drills (pooled second-order models, Equation (5)); circles are the measured condition means (n = 3); predictions of the edge responses are clamped at zero.
Figure 8.
RSM surfaces of (a) Fmax, (b) Tw, (c) Tmax, (d) |BHout|, (e) BRout and (f) composite desirability D as functions of spindle speed and feed for the three drills (pooled second-order models, Equation (5)); circles are the measured condition means (n = 3); predictions of the edge responses are clamped at zero.

Table 2.
Experimental matrix of the first series (33 full factorial, 27 holes) and measured responses. Fmean, Fmax: mean and maximum thrust force; Tw: workpiece surface temperature (point 2); Tchip: maximum chip temperature; Tmax: maximum drill temperature; Deq: aperture equivalent diameter at the entry (in) and exit (out) face; BHin, BHout: burr height at the entry and exit face; BRout: bulging ratio of the 0–300 µm exit edge band. † Chip packing around the drill point recorded during the test.
Table 2.
Experimental matrix of the first series (33 full factorial, 27 holes) and measured responses. Fmean, Fmax: mean and maximum thrust force; Tw: workpiece surface temperature (point 2); Tchip: maximum chip temperature; Tmax: maximum drill temperature; Deq: aperture equivalent diameter at the entry (in) and exit (out) face; BHin, BHout: burr height at the entry and exit face; BRout: bulging ratio of the 0–300 µm exit edge band. † Chip packing around the drill point recorded during the test.
| Exp. | Drill | n(rpm) | f(mm/rev) | Fmean(N) | Fmax(N) | Tw(°C) | Tchip(°C) | Tmax(°C) | Deq,in(mm) | Deq,out(mm) | BHin(µm) | BHout(µm) | BRout(%) |
| E1 | HSS-R | 715 | 0.1 | 39.0 | 39.6 | 25.8 | 43.4 | 96.5 | 6.41 | 6.02 | 14 | 17 | 11.1 |
| E7 | HSS-R | 715 | 0.2 | 32.9 | 33.3 | 24.2 | 31.0 | 100.5 | 6.39 | 6.00 | 6 | 38 | 13.7 |
| E13 | HSS-R | 715 | 0.3 | 35.0 | 35.7 | 26.2 | 43.0 | 112.4 | 6.37 | 6.04 | 4 | 28 | 8.0 |
| E19 | HSS-R | 1520 | 0.1 | 35.6 | 36.8 | 26.7 | 54.0 | 102.6 | 6.16 | 6.04 | 9 | 12 | 1.2 |
| E25 | HSS-R | 1520 | 0.2 | 35.6 | 37.0 | 26.5 | 71.2 | 112.9 | 6.03 | 6.04 | −75 | 21 | 3.8 |
| E31 | HSS-R | 1520 | 0.3 | 37.5 | 38.0 | 27.2 | 82.0 | 119.3 | 6.08 | 5.97 | −6 | 32 | 5.8 |
| E37 | HSS-R | 3030 | 0.1 | 34.2 | 34.6 | 28.5 | 47.7 | 114.2 | 6.47 | 6.10 | 2 | 24 | 9.8 |
| E43 | HSS-R | 3030 | 0.2 | 40.5 | 41.0 | 29.3 | 32.4 | 100.7 | 6.35 | 6.05 | 7 | 20 | 1.4 |
| E49 | HSS-R | 3030 | 0.3 | 42.1 | 43.5 | 30.0 | 81.7 | 107.6 | 6.44 | 6.09 | −25 | −23 | 0.1 |
| E3 | HSS-G | 715 | 0.1 | 34.5 | 37.1 | 31.9 | 56.9 | 84.4 | 5.95 | 5.89 | 3 | 26 | 5.1 |
| E9 † | HSS-G | 715 | 0.2 | 43.6 | 46.1 | 33.0 | 85.2 | 104.3 | 6.01 | 7.00 | 21 | 245 | 85.1 |
| E15 | HSS-G | 715 | 0.3 | 31.6 | 34.0 | 28.6 | 66.2 | 123.0 | 5.93 | 5.99 | 7 | 8 | 2.7 |
| E21 | HSS-G | 1520 | 0.1 | 28.5 | 29.4 | 26.5 | 34.8 | 111.8 | 6.01 | 5.98 | −12 | 23 | 0.4 |
| E27 | HSS-G | 1520 | 0.2 | 30.9 | 31.9 | 29.1 | 37.5 | 106.2 | 5.96 | 6.00 | −12 | 2 | 0.8 |
| E33 | HSS-G | 1520 | 0.3 | 28.9 | 29.6 | 27.0 | 33.8 | 107.6 | 6.01 | 6.00 | 7 | 16 | 4.5 |
| E39 | HSS-G | 3030 | 0.1 | 29.7 | 30.2 | 28.3 | 59.1 | 106.9 | 6.02 | 6.00 | 19 | 23 | 4.6 |
| E45 † | HSS-G | 3030 | 0.2 | 41.9 | 46.2 | 43.4 | 82.3 | 99.2 | 6.03 | 5.97 | 1 | 22 | 6.4 |
| E51 | HSS-G | 3030 | 0.3 | 30.4 | 31.1 | 29.0 | 70.6 | 120.3 | 6.02 | 6.02 | −1 | 27 | 5.2 |
| E5 | Carbide | 715 | 0.1 | 35.2 | 37.6 | 26.3 | 32.8 | 89.1 | 6.39 | 6.35 | 28 | 42 | 19.3 |
| E11 | Carbide | 715 | 0.2 | 44.0 | 47.0 | 37.8 | 85.6 | 104.3 | 6.41 | 6.35 | 37 | −71 | 6.3 |
| E17 | Carbide | 715 | 0.3 | 39.4 | 41.7 | 31.2 | 66.7 | 112.5 | 6.43 | 6.31 | 24 | 75 | 32.7 |
| E23 | Carbide | 1520 | 0.1 | 40.7 | 42.5 | 37.9 | 55.6 | 106.8 | 6.36 | 6.37 | −11 | 91 | 23.4 |
| E29 | Carbide | 1520 | 0.2 | 37.9 | 38.6 | 29.9 | 41.2 | 114.4 | 6.40 | 6.36 | 15 | 59 | 26.0 |
| E35 | Carbide | 1520 | 0.3 | 36.8 | 37.6 | 29.8 | 74.1 | 119.8 | 6.31 | 6.35 | −11 | 152 | 41.5 |
| E41 | Carbide | 3030 | 0.1 | 40.6 | 41.3 | 30.5 | 26.1 | 101.5 | 6.37 | 6.34 | −15 | −41 | 10.5 |
| E47 | Carbide | 3030 | 0.2 | 36.7 | 37.9 | 30.5 | 43.2 | 108.8 | 6.39 | 6.34 | −92 | 12 | 31.4 |
| E53 | Carbide | 3030 | 0.3 | 43.9 | 44.8 | 34.4 | 58.8 | 109.3 | 6.31 | 6.33 | −25 | 34 | 10.8 |
Table 3.
ANOVA of the process responses of the first series (27 holes; type-II sums of squares; PC = percentage contribution; three-factor interaction pooled as error). BRout analysed without E9. Values of p < 0.05 are significant.
Table 3.
ANOVA of the process responses of the first series (27 holes; type-II sums of squares; PC = percentage contribution; three-factor interaction pooled as error). BRout analysed without E9. Values of p < 0.05 are significant.
| Source | FmeanPC (%) | p | TmaxPC (%) | p | TchipPC (%) | p | BRoutPC (%) | p |
| Drill type | 29.6 | 0.029 | 0.0 | 0.994 | 1.3 | 0.725 | 57.8 | 0.003 |
| Spindle speed | 8.4 | 0.258 | 14.5 | 0.095 | 0.4 | 0.898 | 1.5 | 0.709 |
| Feed | 6.9 | 0.318 | 38.0 | 0.011 | 16.5 | 0.058 | 1.2 | 0.748 |
| Drill × Speed | 9.4 | 0.505 | 2.5 | 0.886 | 45.5 | 0.018 | 11.8 | 0.313 |
| Drill × Feed | 18.1 | 0.232 | 5.9 | 0.643 | 12.7 | 0.265 | 4.8 | 0.682 |
| Speed × Feed | 7.0 | 0.626 | 21.0 | 0.144 | 7.6 | 0.480 | 8.8 | 0.435 |
| Error | 20.7 | — | 18.1 | — | 15.9 | — | 14.2 | — |
Table 4.
Hole-edge quality metrics per drill and face (mean ± sample standard deviation over the nine holes of each drill; eight for HSS-G, E9 excluded). Oversize = Deq − Dnom with Dnom = 6.00 mm (HSS) and 6.35 mm (carbide); BH: burr height; BR: bulging ratio; DF: depressed fraction.
Table 4.
Hole-edge quality metrics per drill and face (mean ± sample standard deviation over the nine holes of each drill; eight for HSS-G, E9 excluded). Oversize = Deq − Dnom with Dnom = 6.00 mm (HSS) and 6.35 mm (carbide); BH: burr height; BR: bulging ratio; DF: depressed fraction.
| Drill | Face | Oversize (µm) | BH(µm) | BR(%) | DF(%) | Dmax− Dmin (µm) | Reported hole area (mm²) | Reported peak area (mm²) |
| HSS-R | Entry | +301 ± 166 | −7.0 ± 27.7 | 5.4 | 3.9 | 407 | 17.9 | 2.43 |
| HSS-R | Exit | +38 ± 40 | 18.9 ± 17.6 | 6.1 | 2.6 | 450 | 14.8 | 2.40 |
| HSS-G | Entry | −8 ± 38 | 1.6 ± 10.2 | 4.7 | 3.1 | 387 | 15.9 | 2.36 |
| HSS-G | Exit | −19 ± 40 | 18.4 ± 9.1 | 3.7 | 1.4 | 394 | 13.4 | 2.92 |
| Carbide | Entry | +25 ± 42 | −5.6 ± 39.2 | 7.5 | 4.0 | 406 | 18.6 | 3.01 |
| Carbide | Exit | −7 ± 17 | 39.1 ± 67.5 | 22.4 | 4.6 | 430 | 19.1 | 1.66 |
Table 5.
Percentage contributions of drill type, spindle speed, feed and their interactions to the variation of the responses (full 33 factorial model, three replicates, 81 observations; DF = degrees of freedom; signed BHout).
Table 5.
Percentage contributions of drill type, spindle speed, feed and their interactions to the variation of the responses (full 33 factorial model, three replicates, 81 observations; DF = degrees of freedom; signed BHout).
| Source | DF | Fmax(N) | Tw(°C) | Tmax(°C) | BHout(µm) | BRout(%) |
| Model | 26 | 97.76 | 99.66 | 98.69 | 99.98 | 99.97 |
| Linear | 6 | 58.77 | 46.16 | 57.56 | 12.76 | 28.11 |
| Drill type | 2 | 51.92 | 35.88 | 2.59 | 3.46 | 14.82 |
| Spindle speed | 2 | 5.45 | 6.73 | 9.42 | 7.89 | 7.72 |
| Feed | 2 | 1.40 | 3.55 | 45.55 | 1.41 | 5.57 |
| Two-way interactions | 12 | 19.21 | 27.84 | 26.87 | 52.93 | 36.83 |
| Drill × Speed | 4 | 9.07 | 8.91 | 6.84 | 24.94 | 14.55 |
| Drill × Feed | 4 | 5.20 | 9.00 | 6.80 | 23.12 | 13.89 |
| Speed × Feed | 4 | 4.94 | 9.93 | 13.23 | 4.87 | 8.39 |
| Three-way interaction | 8 | 19.77 | 25.66 | 14.26 | 34.29 | 35.02 |
| Drill × Speed × Feed | 8 | 19.77 | 25.66 | 14.26 | 34.29 | 35.02 |
| Error | 54 | 2.24 | 0.34 | 1.31 | 0.02 | 0.03 |
| Total | 80 | 100.00 | 100.00 | 100.00 | 100.00 | 100.00 |
Table 6.
Optimisation objectives, importance weights and desirability limits (Li, Ui = minimum and maximum of the 81 observations).
Table 6.
Optimisation objectives, importance weights and desirability limits (Li, Ui = minimum and maximum of the 81 observations).
| Response | Symbol | Goal | Weight | Normalised weight | Li | Ui |
| Maximum thrust force (N) | Fmax | Minimise | 3 | 0.158 | 29.6 | 46.6 |
| Workpiece temperature (°C) | Tw | Minimise | 3 | 0.158 | 24.7 | 35.55 |
| Maximum drill temperature (°C) | Tmax | Minimise | 3 | 0.158 | 84.3 | 128.2 |
| Exit burr height, magnitude (µm) | |BHout| | Minimise | 5 | 0.263 | 1.8 | 239.5 |
| Exit bulging ratio (%) | BRout | Minimise | 5 | 0.263 | 0.1 | 83.3 |
Table 7.
Coded regression coefficients of Equation (5) (* p < 0.05, ** p < 0.01, *** p < 0.001).
| Response | β0 | βG | βC | β1 | β2 | β11 | β22 | β12 |
| Fmax (N) | 37.81*** | −4.79*** | 3.20*** | 0.35 | 0.17 | 2.20** | −1.10 | 1.03* |
| Tw (°C) | 26.80*** | 1.79** | 4.02*** | 0.69* | 0.48 | 0.96 | −0.70 | 0.08 |
| Tmax (°C) | 107.53*** | −1.34 | 2.06 | 2.72*** | 6.98*** | −3.05* | 3.46** | −4.38*** |
| |BHout| (µm) | 36.39** | 19.02 | 39.70** | −17.56** | 5.17 | −2.60 | −15.71 | −2.10 |
| BRout (%) | 9.99* | 6.48 | 16.19*** | −5.66** | 1.40 | 2.55 | −8.32* | −1.21 |
Table 8.
The ten best machine-feasible conditions ranked by composite desirability D (measured condition means, n = 3). S: weighted-sum score (Equation (3)); RSM D (rank): composite desirability predicted by the RSM and its rank among the 27 conditions. The complete ranking is given in Table S1.
Table 8.
The ten best machine-feasible conditions ranked by composite desirability D (measured condition means, n = 3). S: weighted-sum score (Equation (3)); RSM D (rank): composite desirability predicted by the RSM and its rank among the 27 conditions. The complete ranking is given in Table S1.
| Rank | Drill | n(rpm) | f(mm/rev) | Fmax(N) | Tw(°C) | Tmax(°C) | |BHout| (µm) | BRout(%) | D | S | RSM D (rank) |
| 1 | HSS-G | 1520 | 0.2 | 31.1 | 27.2 | 102.5 | 1.8 | 0.8 | 0.867 | 0.882 | 0.712 (8) |
| 2 | HSS-G | 1520 | 0.1 | 30.3 | 26.5 | 105.0 | 22.9 | 0.4 | 0.852 | 0.869 | 0.807 (2) |
| 3 | HSS-G | 1520 | 0.3 | 30.4 | 26.7 | 107.9 | 16.0 | 4.6 | 0.825 | 0.848 | 0.682 (12) |
| 4 | Carbide | 715 | 0.1 | 34.6 | 25.4 | 91.8 | 42.0 | 19.5 | 0.808 | 0.811 | 0.573 (20) |
| 5 | HSS-R | 715 | 0.2 | 35.8 | 24.9 | 98.9 | 37.9 | 13.6 | 0.796 | 0.805 | 0.679 (14) |
| 6 | HSS-G | 3030 | 0.1 | 31.8 | 28.5 | 108.0 | 22.8 | 4.6 | 0.777 | 0.801 | 0.769 (5) |
| 7 | HSS-G | 715 | 0.1 | 38.9 | 29.8 | 86.0 | 26.2 | 5.0 | 0.758 | 0.790 | 0.784 (3) |
| 8 | HSS-R | 1520 | 0.1 | 39.1 | 27.4 | 105.6 | 12.3 | 1.2 | 0.744 | 0.780 | 0.812 (1) |
| 9 | HSS-R | 715 | 0.1 | 40.6 | 25.8 | 100.9 | 17.0 | 11.3 | 0.732 | 0.770 | 0.779 (4) |
| 10 | HSS-R | 1520 | 0.2 | 38.0 | 26.0 | 111.4 | 21.2 | 3.8 | 0.731 | 0.773 | 0.718 (7) |
Table 9.
Weight scenarios (weights in the order Fmax, Tw, Tmax, |BHout|, BRout; S1 = baseline) and the corresponding optima. Grid A: drill, speed (rpm) and feed (mm/rev) with measured D; Grid B: RSM-grid optimum with predicted D.
Table 9.
Weight scenarios (weights in the order Fmax, Tw, Tmax, |BHout|, BRout; S1 = baseline) and the corresponding optima. Grid A: drill, speed (rpm) and feed (mm/rev) with measured D; Grid B: RSM-grid optimum with predicted D.
| Scenario | Weights | Grid A optimum | D | Grid B optimum | D |
| S1 | (3, 3, 3, 5, 5) | HSS-G, 1520, 0.2 | 0.867 | HSS-R, 1325, 0.100 | 0.814 |
| S2 | (1, 1, 1, 1, 1) | HSS-G, 1520, 0.2 | 0.836 | HSS-G, 1125, 0.100 | 0.793 |
| S3 | (1, 1, 1, 5, 5) | HSS-G, 1520, 0.2 | 0.931 | HSS-R, 1650, 0.100 | 0.891 |
| S4 | (5, 5, 5, 1, 1) | Carbide, 715, 0.1 | 0.816 | HSS-G, 945, 0.100 | 0.763 |
| S5 | (0, 0, 0, 1, 1) | HSS-G, 1520, 0.2 | 0.995 | HSS-R, 2595, 0.100 | 0.999 |
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content. |
© 2026 by the authors. Licensee MDPI, Basel, Switzerland. This article is an open access article distributed under the terms and conditions of the Creative Commons Attribution (CC BY) license (http://creativecommons.org/licenses/by/4.0/).
Copyright: This open access article is published under a Creative Commons CC BY 4.0 license, which permit the free download, distribution, and reuse, provided that the author and preprint are cited in any reuse.