Abstract
The performance of a lithium-ion battery cell depends on numerous manufacturing factors. During the production ramp-up, variations in these manufacturing parameters influence the final performance of the battery cells. However, the correlation between cell performance and the influencing parameters remains obscure. To address this gap, this comprehensive review investigates which manufacturing factors regulate cell performance, how they are currently monitored and where the critical knowledge gaps lie. The key performance indicators (KPIs) reported in the literature were identified through a rapid review (RR) approach. Factors that were not explicitly reported as applicable across lithium-ion chemistries were re-examined to assess applicability to the most widely used chemistries. These factors were then categorised by their properties, and the analysis showed that dimensional features constitute the largest group among the distinct manufacturing factors affecting lithium-ion battery cell performance, based on the number of variables identified. Despite this finding, limited research has attempted to establish a quantitative relationship between performance and dimensional features. Furthermore, the influence of tolerance stack-up on the electrochemical performance remains unexplored in the existing literature. This gap indicates the need for a structured digital approach capable of linking dimensional measurements, tolerance interactions and cell performance outcomes during production ramp-up.
Keywords: 
;  ;  ;  ;  ;  ;  

1. Introduction

The fast growth of electric vehicles (EV) has accelerated the need for expeditious and reliable development of EV battery cells. Lithium-ion (Li-ion) is the most widely used type of battery cells in EV at present [1]. During the early production phase of Li-ion batteries, variations are very common and these deviations have direct impact on cell performance. Nevertheless, the relationship between cell performance and manufacturing variations is still poorly understood. As a result, the performance of the battery cells are not satisfactory during ramp-up and the manufacturers face high scrap rates as they have to rely trial-and-error methods to get the optimum result [2]. To mitigate this problem, it is essential to establish a quantifiable relationship between dimensional variations and battery cell key performance indicators (KPI). This comprehensive review is a part of a larger project aimed at bridging the gap between dimensional variations and key performance indicators. In this review-based article, current knowledge on manufacturing variation and its impact on battery cell KPIs, present practice in the new product introduction (NPI) phase of battery cells, and potentiality of digital integration within EV cell manufacturing system has been reviewed.
This article is structured around three guiding questions: (1) Which key performance indicators are used for evaluating the performance of EV battery cells, and how are these KPIs influenced by the manufacturing process? (2) Which type of factors are the largest in number that influence the performance, and how are these factors being monitored and controlled conventionally? and (3) What modern digital approaches (e.g. cyber-physical systems (CPS), digital twins) have been applied to manage the variations of these factors in EV cell manufacturing, and do they provide sufficient evidence that a dimensional metrology-driven cyber-physical system or digital twin would be an effective solution for aiding the quality maturation of Li-ion cells? Before delving into deeper discussion, some of the terminologies have been elaborated first for better understanding.

2. Theoretical Framework

2.1. Overview of Battery Cells

A lithium-ion battery is a battery pack that consists of a cell and a circuit [3]. Battery cells are the core part of a pack. Those cells are classified according to their geometry and chemistry. Three forms of battery cells are most commonly used. They are: cylindrical, prismatic, and pouch type. Cathode, anode, separator, and electrolytes are present in all of those form factors.
  • Cylindrical Cell: As its name denotes, it is cylindrical in shape. The case of cylindrical cells is made of stainless steel, with three standard sizes (18650, 2170, and 4680) [3]. The first two digits indicate the diameter, and the latter digits indicate the height of the cells. Due to their standard sizes and ease of manufacturing, cylindrical cells have gained popularity among EV manufacturers.
  • Prismatic Cell: The outer shell of prismatic cells is made by deep drawing aluminium sheets. These cells are popular among the mobile phone manufacturers. Flat jelly rolls or stacked electrodes are used in prismatic cells [4].
  • Pouch Cell: The casing of pouch-type cells is made of aluminium sheets. Their sizes and shapes vary according to their application [3]. For this cause, this type of cell is mostly used in devices where irregular battery shapes are required.

2.2. State-of-the-Art Manufacturing Process

The current state-of-the-art manufacturing process of Li-ion batteries consists of three major processes: electrode manufacturing, cell assembly, and battery activation [5].

2.2.1. Electrode Manufacturing

Electrode manufacturing starts in a dry chamber where the active material and conductive agent are mixed according to weight ratio [6]. The binder powder and solvent are mixed separately to make the binder solution. After a dry mixture of active material and conductive agent is prepared, a binder solution is made to make a slurry. The cathode slurries are mainly dissolved in N-Methyl-2-pyrrolidone (NMP), and the anode slurries are primarily dispersed in deionized water. Preparation of a uniform electrode slurry is done in a planetary mixer, and viscosity is observed as it is one of the key quality parameters. The slurry is then degassed and buffered for 24-48 hours before use in coating. To coat it, a tandem coating machine or a slot die is used in a mass production method to spread a slurry on a substrate film, while surface cracks are inhibited by using a multi-zone dryer to evaporate the solvent. NMP is condensed and distilled to recover as it is a toxic solvent. After coating, the electrode is calendered, or pulled through a pair of rollers to decrease thickness by compression, which intensifies the particles into the slurry film and, therefore, increases volumetric energy density and enhances electrical conductivity. The electrode web is then slit or cut to size or into various shapes as per the requirement. Quality control is momentous when manufacturing electrodes, and consistency, porosity, and the lack of flaws are essential. The complexity associated with manufacturing processes, such as dynamic mixing and solvent evaporation, can lead to defects like particle agglomerations, air bubbles, and flaking or buckling edges, particularly in high-speed, wide-web coater operations. These defects may lead to issues such as lithium plating or overheating, which can significantly impact cell performance.

2.2.2. Cell Assembly

The assembly of the cell begins with computer-controlled notching with a laser where electrode tabs or single sheets are cut to size from the electrode web. This procedure is critical because inferior slitting results in separator protrusion, electrical stress concentration, and performance degradation [7]. This may cause the battery to explode in extreme cases. During this stage, the tube is also carefully inspected for mechanical or thermal deformation and surface contamination in parallel. Stacking and welding processes are conducted subsequently. Although ultrasonic welding is used to attach the tab and collector, laser welding is gaining popularity for its speed and non-contact properties [8]. After welding and stacking, the cell stack (also known as a jelly roll for cylindrical cells), is fixed with tape to avoid displacement. After that, it is heat pressed and assessed by accurate thickness measurement [6]. Electrical insulation between the anode and cathode is checked by Hi-Pot (high potential) measurement to find any manufacturing defects. The stack is modelled as a resistor-capacitor (RC) circuit, and the insulation quality is characterised by measuring the leakage current over a certain period (for example, 5 seconds). Currents higher than 1 mA represent a possible failure mode, separator crack, or metal contamination.

2.2.3. Battery Activation

This process is often addressed as cell finishing or formation. It is a critical step in cell manufacturing that encompasses formation, ageing, and grading. The formation stage begins with high-temperature soaking, where the electrodes are immersed in electrolyte at nearly 45 degrees Celsius [6]. Then they go to special racks for the initial charging. During the first charge, the crucial protective layer, known as solid electrolyte interphase (SEI) is formed in the anode surface, which prevents the anode from conducting unwanted chemical reactions. During the initial charging, large cells may generate gas that is allowed to escape later in a controlled environment. The second or third filling of the electrolyte is generally done after charging, together with laser cleaning of the fill port and ultimate closing by laser welding. Final weighing and measurement checks, together with a helium leak test, are done.
The wetting and formation process usually takes 3–7 days [9]. After that, a variety of longer ageing phases may take up to two weeks in duration, consisting of rest periods at both high temperatures and room temperature, application of various current/voltage profiles, and open-circuit voltage testing that assesses self-discharge behaviour. High rates of self-discharge could signify internal defects. Finally, in the last stage, the cells are graded according to voltage and internal resistance, wrapped in Polyethylene Terephthalate (PET) tape, undergo dimensional, insulation, and thickness testing, are sorted by performance, and prepared for shipping.

3. Methodology

3.1. Identification of the Key Performance Indicators of EV Battery Cells

The perception of key performance indicators (KPI) has become central to understanding and managing the performance of EV battery cells across both product and process dimensions. To find out the KPI of EV battery cells, a systematic rapid review (RR) approach was adopted. Firstly, as lithium-ion batteries are the most widely used batteries in electric vehicles, those were selected as the targeted battery type for this study. Scopus was selected as the research database for searching as this is one of the most prominent databases for finding technology-related publications. The search keywords were “Battery Cell Performance Indicators” so the title and abstract with the same keyword might come out as a search result. Given the rapid evolution of EV battery technologies, the primary search window was restricted to the last five years, similar to a recent review based article on the state of health (SOH) of batteries that explicitly frame their analysis over this horizon [10]. Then the published and English journals were filtered, which reduced the result from 612 to 366. After checking the title, 140 papers were considered for abstract review. Finally, abstracts of the papers were checked to ensure that the papers explicitly mention the terms “Key Performance Indicator”, “Indicators” or “KPI” in the abstract. Checking the abstracts helped to bring down the quantity to 23.
After going through the full text of the remaining 23 articles, 10 studies were excluded. Only the studies that recognized one or more metrics as KPI of Li-ion battery cells (not packs or modules) were included for further studies. The reasons for exclusion are mentioned in the Table 1.
The summary of the rapid review (RR) steps is illustrated in Figure 1.
From the remaining 13 research papers, 16 key performance indicators were found which are detailed in Table 2.
After identifying all the influencing factors, additional literature were reviewed for the factors that had not been declared as cross-chemistry applicable, to ascertain whether the correlation could be generalized to other commonly used lithium-ion battery chemistries. As NMC, LFP and LMO batteries are most suitable to be used in electric vehicle applications [34], these three chemistries were considered as potential candidates for cross-chemistry check. However, the factors which are common for all chemistries (e.g. cost) have been contemplated as universal for all chemistries. After that, each of those factors were categorized into dimensional, process, material, and external according to their nature and role in the manufacturing operation. The summary of the findings are shared in Appendix Table A1.

4. Results and Discussion

4.1. Manufacturing variables affecting the KPIs

As the KPIs had been found, the next step was to find which manufacturing variables drive those performance indicators. This section is about describing the drivers of those KPIs. Each of the KPIs is addressed and detailed how they are controlled by manufacturing variables.
  • Capacity: Cell capacity can be evaluated mostly by discharging capacity in Ampere-hour (Ah) after a full charge unless otherwise specified [35]. Broad and Fly [36] used a pseudo-2D model and simulated that in case of nickel manganese cobalt (NMC) cathode and silicon-graphite anode, the capacity changes in proportion to electrode height which is a dimensional feature. The same result occurs when the width of the electrode (length of the jelly roll) changes because it alters the amount of active material. The model also theoretically demonstrated that increase in coating thickness in the anode increases the capacity as more coating means more Graphite/Si particles. After calendering, the electrode is back to its original thickness. So, active material increases and porosity decreases. From this paper, it can be said that coating, calendering, and electrode cutting operations need strict dimensional control to ensure desired performance. In another study, it was shown with the help of an ML model and a pilot calendering operation that coating weight, coating thickness, density, porosity, roll gap and roller temperature are the five calendering factors that affect a cell’s capacity, while coating weight and thickness are the most influential and roller temperature is the least [37]. Apart from that, it was demonstrated that during slurry formation and mixing of NMC battery cells, if the ratio of carbon black and binder (CB:B ratio) is increased, carbon black prevents isolation, increases solid-liquid inter-facial area and so, the capacity increases as well [38]. Also, inadequate synthesis of electrode causes phase impurities and uneven distribution of element and thus reduces capacity [39]. It was also mentioned that at moderate speeds, surface-engineered graphite coated with just 1 weight percent aluminium oxide (Al2O3) exhibits a reversible capacity of roughly 337.1 mAhg−1. The electrochemical activities of Li-ion cells occur mostly in the geometrical regions. Therefore, when the battery is charged, the lithiation of the anode occurs mainly in the areas that are in line with the cathode coating. A slight shortage or misalignment could result in a reduction of cell capacity. To mitigate the problem, the anode is intentionally kept longer than the cathode, which can be defined as overhang. The exact overhang depends on the cell type [40]. It was found that in a commercial 8Ah LiFePO4 battery, the overhang is about 5.7% of the active cathode area[41]. But if the anode is too long, it causes capacity loss gradually in the long run as Li+ ion deposition increases in the inactive area, as mentioned in another critical review [42].
  • Cycle life: Cycle life is defined as the number of discharge cycles a battery cell can deliver before its capacity is depleted at 80% of the initial capacity [43]. Choice of solid electrolyte interface (SEI) formation method affects the cycle life of batteries. Research on two types of formation protocol substantiated that fast formation spends less time at low negative-electrode potentials and more time at high voltage, which promotes formation of a more passivating SEI [44]. This consumes more lithium during formation, creating a strong and protective SEI. This type of SEI suppresses electrolyte reduction, pore clogging and lithium plating. For this reason, fast-formation cycle lasted over 100 cycles more than the baseline formation cells before reaching End of Life (EOL).
    Weld tab thickness plays a dominant role in cells’ life-cycle [45]. Thicker weld tabs made from current collectors are about 100-150 micro metres which is higher than the current collectors (thickness ranging from 10-100 micro metres). This difference causes local stiffness and stress concentrations in the jellyroll that initiate bending, cracking, and loss of adhesion, while foil tabs are mechanically stable and show no deformity even after 2000 cycles. It was also exemplified that a welded tab creates pressure inhomogeneities which leads to local lithium deposition of anode and results in capacity drop leading to lower cycle life. In contrast, avoidance of inhomogeneity with foil tabs and using multiple tabs result in 26.8% longer cycle life.
    Anode-cathode overhang also plays an important role to determine the cycle life [46]. Cathode overhang is detrimental to cyclability and safety because lithium can be plated on the upper part of the graphite anode due to over supply of lithium. It showed almost half-cycle life than a cell with anode-cathode overhang. Distorted roundness of jelly-rolls are liable for electrode defects and shorter cycle life for lithium iron phosphate (LFP) cells. It was also evinced that heterogeneous anodes cause more non-uniform reactions, resulting from locally concentrated current and heat distributions, which shortens its cycle life.
  • Charging Capability & Fast-charging Performance: By experimenting with a pouch cell of NMC and graphite anode, it has been demonstrated that fast charging performance depends on the amount of electrolyte filled inside the cell. If electrolyte filling is inadequate during manufacturing, charging time becomes longer [47].
    Also, it has been demonstrated that anode slurry mixing is a critical manufacturing parameter for fast charging performance by linking mixing conditions to micro-structure and lithium plating in lithium-ion cells [48]. The authors found that high-intensity planetary mixer causes graphite particle abrasion that results in a non-uniform pore network which reduces charging capability. In contrast, gentler dissolver-based mixing enables a more homogeneous structure and supports better fast-charging performance.
    Calendering pressure also influences the charging capability [49]. It was clearly demonstrated with different samples that higher calendering pressure exerted on graphite anodes lessens the electrolyte flow, increase tortuosity of Li+ ions and thus minimizes the charging capability.
    Electrode thickness plays a pivotal role in regulating the charging capability of a battery cell. Although a thicker electrode improves capacity, it hinders the efficient movement of ions and increases internal resistance during fast charging [49]. On the other hand, cells made from thinner electrodes have increased fast-charging performance but reduced capacity. So, the authors recommended to ensure optimum dimensions to obtain the desired capacity and fast charging performance. Also, they emphasised ensuring proper porosity of the electrodes as low porosity reduces electrolyte volume and hampers ionic transport which reduces charging capability.
  • Cost: EV battery cell cost is dominated by material cost and yield rate. Orangi and Strømman[50] demonstrated that cathode active material costs almost 57% of the total cost and almost 30% of the whole product. Apart from that, with the increase of scrap and rejection rate, the cost of the cell increases non-linearly. Here, scrap means the semi-finished goods which are wasted in the production line, and the rejected products are those which fail in the testing process after the production. Moreover, higher production volume lowers cathode active material price and spreads fixed costs. It was also observed that labour, machinery, energy and scrap cost are higher than most other costs in battery cell production. After observing costs of 9 countries, the authors concluded that labour cost is the most important factor in this industry. To control the labour cost, manufacturers are patronizing automation to reduce the dependency on manual labour.
    Another process-based cost modelling demonstrated that increasing yearly production output spreads the fixed cost and reduces per unit production cost [51]. Also, thickening the electrode sheets per cell lessens roll-to-roll cycle time per kWh. In addition, high capacity electrode materials increase Wh per cell and reduce electrode count per kWh, raising roll-to-roll capacity. It was mentioned that lower scrap rate increases saleable output and effective capacity utilization and thus, reduces cost.
  • Energy and Energy Density: There are three driving variables that set the energy of a battery cell. Firstly, the cell diameter changes jelly-roll length, active material volume per cell, number of cells that fit into the installation space, and interconnection constraints, which together determine total battery energy [28]. Therefore, energy rises and then falls as diameter increases and decreases due to packing and spacing trade-off. Also, cell height determines active material volume per cell and is limited by venting gap and cooling plate. Energy is calculated from jelly-roll geometry including coating height and total active material volume. Aside from that, cell housing materials govern wall thickness, cell internal volume, spacing for safety, and packing efficiency, which all change how much active material fits in the battery system and thus determine energy of the cell.
    Developing cell chemistry is one of the major methods to enhance energy density [52]. Apart from that, cell design parameters also influence this KPI. For instance, lowering the ratio of negative and positive materials (N:P ratio) by depleting the thickness of anode increases energy density because it decreases the fraction of inactive material compared to active material in the stack in same weight and volume. Alternatively, thicker electrode for the same amount of material results in excessive porosity. Moreover, formulation control has significant impact on energy density. If wt% of active material is increased in lithium cobalt oxide (LCO) cathode, it reduces coating thickness and thus increases energy density. In a different research related to design optimization, it was stated that the cathode thickness determines how much active material is stored per electrode and how many current collectors and separators are needed [53]. Variation in thickness changes both total mass and volume of active vs inactive materials and thus alters energy density. In contrast, ensuring optimized thickness improves energy density. Also, it was mentioned that anode thickness sets lithium-storage capacity and inactive mass. Too thick adds dead mass; too thin limits usable cathode capacity. Similarly, negative current collector thickness (i.e. copper foil) adds mass but no energy. So, increasing collector thickness reduces gravimetric energy density. For the same reason, tight control of separator thickness is essential to reduce cell-to-cell variation in energy density. In that research, the authors observed that anode particle size was reduced from 12.5 to 0.65 micro metres which increased energy density by improving lithiation efficiency and enabling better electrode utilization. Therefore, it is essential to ensure optimum particle size while sourcing or manufacturing. In case of NMC, coating mass loading, which is determined by the slurry density and wet coating thickness, directly controls how much active material is deposited per unit area [54]. Higher mass loading increases the amount of lithium-storage material in the cathode, which raises discharge capacity and thus volumetric energy density.
    As mentioned earlier, improper synthesis of cathode, which causes structural defects and phase impurities, also decreases energy density apart from capacity [39].
    A review based research found that higher Nickel content in NMC cathode increases energy density [55]. So, cathode chemistry is a crucial parameter to be controlled to get the desired energy density for NMC.
  • Internal resistance (IR): Internal resistance depends on multiple manufacturing parameters. There are three reasons behind the deviation of IR during manufacturing [56]. The battery cover positive terminal and negative terminals has different resistance in different caps that causes difference in internal resistance. Around 20% difference of resistance between batches was found in the cited study. In addition, it was observed that poor slurry mixing causes active material, conductive agent and binder to agglomerate, producing high resistivity in the composite layer and high interface resistance to the current collector, which increases electronic resistance inside the pole group. Finally, electrode coating speed plays a vital role in determining the IR of the cell. The authors observed that for the same slurry, changing coating speed alters the internal blockage of the polar sheet, which changes composite-layer resistance. So, under identical slurry conditions, higher coating speed produces lower composite-layer internal resistance. In another study with NMC cathode, the IR was divided into two types: ionic, and charge transfer [57]. It was shown that ionic resistance increases with cathode thickness because ions must travel longer distances in pores, while charge-transfer resistance decreases because active surface area increases.
    Even if all of those mentioned process are done properly, the welding of the collector-to-tab join might increase the internal resistance [58]. So, the researchers emphasised the need for precise welding of thin foil and tab. It has been claimed through theoretical analysis that resistance of the weld tab and collector varies with the variation of seam width and length [59]. Although the authors did not explain how the seam dimensions were measured, it is worth investigating further from a metrological point-of-view.
  • Open-circuit Voltage & Voltage: Lithium-to-transition-metal ratio plays a vital role to tune the voltage of Nickel based cathode cells [60]. During cathode synthesis, increasing the lithium-to-transition-metal ratio reduces Ni defect at Li sites formed during synthesis. It lowers the voltage at which the cathode undergoes its high-voltage structural transition. A higher concentration of Ni defects stabilizes the cathode lattice and raises this transition voltage, producing a higher high-voltage plateau.
    Other than this variable, no manufacturing or material variable was found in any other paper that regulates the voltage.
  • Power Output: It has been shown with NMC cells that increasing the percentage of active materials reduce cathode coating thickness and increase specific surface area, which shortens Li+ diffusion distance and reduces reaction overpotential, lowering discharge time. As discharge time decreases, power output increases [61].
    Another study demonstrated that thicker electrodes create longer diffusion distance and stronger concentration polarization, which increases internal resistance and causes larger ohmic drops; hence, power output decreases especially at high discharge rates [62]. Conversely, thin electrodes shorten the diffusion paths and ensure more uniform Li-ion concentration and lead to lower resistance, lower polarization, and higher operating voltage during discharge. It enables higher and more stable power output.
  • Power density: Power density can be defined as the power available per unit volume [63]. There are several manufacturing variables which determine the power density of a battery cell. It has been demonstrated with a physics-based electrochemical model that increasing cathode thickness reduces the power density of battery cells but increases energy density [64]. It happens due the longer diffusion path for the Li+ ions and large underutilized area because of high thickness. The authors emphasised ensuring the optimal thickness to ensure a balance between power density and energy density.
    Manufacturing variations in anode particle size, cathode porosity, anode and cathode thickness, anode current collector thickness and separator thickness were found to be the dominant drivers of power density in lithium manganese oxide (LMO) cells [53]. The parameters which have a tendency to fluctuate during electronic coating, calendering, or lamination directly affect ionic transport, electronic resistance, and reaction kinetics inside the porous electrodes. Due to this reason, their variabilities produce significant cell-to-cell variations causing many cells to fall outside the acceptable power-density limits.
  • Safety: Safety is one of the most prioritized KPI to battery manufacturers [65]. Each and every part of the cell is needed to be designed and manufactured considering safety as the most decisive factor.
    Apart from reducing cycle life, improper anode-cathode overhang may cause short circuit due to lithium deposition and cause safety risk [46]. In order to ensure safety of cells, anode cathode overhang is required to be kept within tolerance range.
    Electrolyte composition is another variable that controls the stability of the electrochemical system and reactions which is essential for operational safety [64].
    Ensuring the purity of metal particles is also essential to warrant the safety of the cell. Even any extraneous metal particle of 10 microns may cause short circuit by puncturing the separator [66].
    Welding tab and welding process have impact on safety too. Thickness of the weld tab in the negative terminal must be kept within 50%-60% of the case thickness, as it may pierce the case if it is higher [67].
    In addition, the strength of join between current collector and weld tab depends on weld penetration depth. It is claimed that insufficient penetration leads to under-weld problem which can be detected by its low joining strength [8]. Conversely, excessive melting due to extra power causes base material melting, which results in underfill and sometimes burn through that compromises safety.
  • Temperature: Electrodes play an important role to determine the temperature of a battery cell. It has been shown in experiments with lithium nickel oxide (LNO) cathode that larger particles in the negative electrode increase solid-state diffusion limitations and surface overpotential, causing higher polarization and more ohmic heat generation [68]. On the other hand, smaller particles delay reaching cut-off voltage so heating gets delayed. It has been shown that increasing particle size by 20 micro metres shows significant heat rise. Some electrodes even rise more than 135 °C and melt the separator. Also, it was demonstrated that since lower porosity means more active material, it leads to higher temperature rise. Furthermore, thinner electrodes heat up less as they have lower concentration over-potential and thus lower temperature rise. But the rise of temperature is not the same in different chemistries. With the help of thermography, it has been exhibited that lithium titanate (LTO) anode batteries have lower surface temperature rise than battery cells with graphite anode since LTO anode has higher conductivity than graphite [69]. Also, graphite anodes have thicker SEI which increase resistance. Additionally, width of LTO weld tab is much higher than LFP and NMC cells. Thus, it reduces the resistance and heat generation. As this phenomena follows Pouillet’s law, this correlation of tab width and temperature is applicable for all chemistries.
    It was further shown with a thermochemical model that lowering porosity increases tortuosity and electrolyte transport resistance, which enhances the Li+ concentration gradient and electrolyte potential, and therefore produces an increase in the internal resistance. The increase of internal resistance magnifies joule heating inside the cell [70]. The amount of material controls the porosity. So, the authors suggested that by controlling active material percentage the maximum temperature can be controlled. Although the experiment was done using NMC cells, the authors claimed that this model is extensible to other battery chemistries.
  • State of Health & State of Charge: Even though state of health and state of charge have been recognized as performance indicators, no literature showed direct measurement of these two performance indicators. Rather, these two are calculated in numerous methods with the help of other performance indicators. For instance, SOH is estimated by health indicators which have been classified into capacity related, internal resistance related, temperature related and charge-discharge curve feature [71]. Similarly, SOC can be calculated using the measured battery current and voltage along with capacity and internal resistance and an extended kalman filter (EKF) algorithm [72]. These studies demonstrate that these two KPIs are compound performance indicators and hence dependent on other KPIs. So, for the ease of analysis, these two performance indicators will be kept out of consideration in the next part.
In order to identify the largest category of affecting factors reported in the literature, duplicate factors were removed and each of the unique factors were kept under consideration. Then the total quantity of each factor type was counted. It was observed that out of 46 unique affecting factors, there are 18 dimensional factors; this is the largest group. External factors was the group with fewest items. It is visualized in the pie chart shared in Figure 2.
The analysis shows that dimensional features emerged as the largest group among the unique manufacturing variables affecting lithium-ion battery cell performance according to the reviewed literature. Also, all the dimension-performance correlations are chemistry agnostic. Therefore, regardless of the battery chemistry, careful optimization and stringent control of these factors during production ramp-up may facilitate defect minimization and quality assurance while simultaneously reducing production ramp-up time and escalating the progression of quality maturation. However, it remains obscure whether the dimensional features and impact of their associated tolerances has been sufficiently understood. Also, it is not evident whether the current dimensional measurement methods have evolved enough to capture and utilize the information during manufacturing. In the next section, the current measurement practices and their limitations will be discussed.

4.2. Measurement and Quality Control Practices During NPI

New Product Introduction (NPI) refers to the sequence or step of activities that an organization executes to commercialize a specific product and it includes activities required to ensure product manufacturability [73].
tab:affecting-factors shows that the identified dimension-performance correlations are chemistry-agnostic. So, it can be hypothesized that regardless of the cell chemistry, Li-ion battery performance depends on geometrical features. When the production is matured enough, the manufacturers have steady machine set-up, known procedure and stable quality control protocol. However, in case of new products, the cell format, jigs and fixtures, materials, and machines are mostly new. In contrast to mature production systems, there is less prior knowledge of how a design can be produced at an industrial scale in case of manufacturing a new product [74]. Also, there is a significant difference between an engineering prototype and a factory prototype. The engineering prototype is developed in a lab to validate the product, whereas a factory prototype is developed in a full-scale production system in order to validate the whole process and the industrial product. This is particularly true for lithium ion battery cells because most of the batteries face challenges during scalability where new process chemistries and form factors are introduced. And it gets further complicated by the fact that the KPIs are not observable during the production but emerge only after formation and ageing processes that take several days or weeks to complete [9].
During NPI, battery manufacturers rely on a combination of physical and digital measurements to assure product quality. For instance, coating thickness, coating weight, porosity proxies, and web width are routinely measured to assess uniformity of slurry and calendering [54]. Optical sensors and electromagnetic measurement methods are most widely used for the inspection of intermediate products. Acoustic methods like ultrasonic inspections are avoided as it requires surface contact, which may damage the surface [75]. After the formation is finished, capacity, internal resistance and open-circuit voltage are measured for grading and quality classification [24].
Although the dimensional measurement infrastructure is thorough and extensive, it is aimed for confirming conformance rather than diagnosis and forecasting the future impact. The studies mentioned above indicate that manufacturing metrology in battery cell production is mainly designed to identify whether certain dimensional features lie within the tolerance range, with limited emphasis on quantifying the impact of the dimensional distributions to downstream performance metrics.
While this gap may have limited impact on mature bulk production, it poses significant problems for the new products during the ramp-up phase. Production ramp-up can be defined as the time between the completion of development and the time to reach full capacity utilization [76]. Due to rapid product lifecycles, manufacturers are forced to reduce the time-to-market (development time) as well as reaching to maximum production capacity. During the ramp-up period of EV battery cells the situation gets more complicated as the process settings, materials and equipment are frequently altered to get the desired result. In this circumstance, the manufacturers are bound to rely on the heuristic trial-and-error method, or by operators’ experience and prior knowledge which can culminate in the scrap rate up to 40% [2].

4.3. Digital Twins and CPS in Cell Manufacturing

Digital twin can be defined by a virtual representation of an existing physical system which acts as a mirror representative of the system to analyse the operation [77]. Data synchronisation and information sharing between the digital twin and the physical counterpart allow for the accurate portrayal of the physical system in cyberspace. There are significant advantages to have a digital representation of the physical object of interest throughout its whole life-cycle, including the stages of development, manufacture, servicing, and disposal. Compared to other fields, digital twin has more widespread application in manufacturing.
On the other hand, cyber-physical system (CPS) can be elucidated as a complex and multifaceted system that combine the physical and computer world through association of 3C: Computing, collaboration and control [78]. Among other functions, CPS offers dynamic control, information feedback, and real-time sensing. Physical and computer processes have close connections and feedback loops, making them extremely interdependent. In this manner, real-time communication and cyber-physical integration are accomplished to monitor and manage physical objects in a dependable, secure, cooperative, robust, and effective manner. Although the concept is derived from embedded systems, the term describes a complex system that could not be properly described with the conventional information technology (IT) terminology. Cyber-physical system (CPS) and digital twin (DTw) both bridge the physical and cyber worlds, but their focus is different. CPS, which was proposed earlier and emphasised in Industry 4.0, is more of a scientific category, while DTws, popularized after 2012 by National Aeronautics and Space Administration (NASA) and the US Air Force, are more engineering-oriented. Both use cyber–physical interaction for improved management of physical systems, but the distinction is that the CPS emphasises computing, collaboration, and control (3C) with one-to-many links, whereas DTw emphasises detailed virtual models with one-to-one mapping. In CPS, sensors and actuators are considered as core components. In contrast, models and data are central in digital twins. Though their components differ, both operate at unit, system, and system-of-systems levels. The bottom line is, both of those can improve the manufacturing through optimized, smart solutions if they can be utilized through the proper application of modern IT.
Like other fields of manufacturing, plenty of research has been done on application of digital twin and cyber-physical system in battery cell manufacturing. For instance, a digital twin was created for the optimization of a flexible lithium-ion battery cell stack formation machine for production ramp-up [79]. It was analysed through the lens of cause-effect relationships in machine commissioning, which is yet to be understood well. The framework comprised a kinematic process model, a web tension simulation model, and a fundamental virtual control system to allow for low-risk virtual testing of the process parameters. The virtual control system also established the relationship between the web tension model and a kinematic process model. Validation against experimental data had been conducted and acceptable accuracy was achieved, indicating potential for reducing commissioning time and material waste. However, the study was confined to a single machine and a single quality-critical variable and doesn’t incorporate the relationship of dimensional variation and cell level performance.
In another literature, a data-driven (CPS) was proposed for lithium-ion battery manufacturing using quality gates and machine learning in order to link the intermediate product features (IPFs) with final product properties (FPPs) [80]. A case study on pouch cells demonstrated the system’s capability to predict future performance and reduce the amount of scrap by ensuring early rejection of defective cells. The paper has a strong structured framework and demonstration of predictive quality management. However, it is limited by a small dataset, focused on a single chemistry, and single-target modelling. Its applicability to large-scale or multi-chemistry contexts remains unproven.
In an exploratory study, a structured framework was presented for identifying, prototyping and selecting digital twin applications in battery cell manufacturing [81]. The authors identified three areas of digital twin application by conducting expert workshops, interviews and observational study. Their findings indicated that machine twins facilitate real-time monitoring of processes and ensure optimum process control. Product twins ensure predictive quality assessment and traceability, while the building twins ensure the optimum logistics through simulation and effective communication. Although the paper outlined an interactive digital twin system, it lacks in-depth analysis in standardization of quality parameters, in-line measurement validation and uncertainty management.
Another vast research provided valuable insights into how a digital twin can serve as a semantic information model by linking raw materials, interim products, sub-assemblies, and final cells, despite being based on a conceptual framework [82]. The research collected 209 quality parameters and categorized those into 4 types such as product features, process parameters, equipment features and ambient condition. Although this structured approach can be considered as a valuable foundation for integrating design and manufacturing, this research remains hypothetical and lacks validation in real-time industrial scale production. Moreover, it did not specify the critical metrological features, their tolerance limits, or the mechanism by which the measured geometry would be captured and integrated to the digital twin. Consequently, the framework remains conceptual with insufficient technical detail to support dimensional traceability or to establish quantitative links between dimensional variations and key performance indicators.

4.4. Gap in Existing Literature

Existing literature shows that there has been attempts to utilize digital systems to measure and control the manufacturing variables in EV battery manufacturing, yet very few of those addressed all the vital dimensions and their impact on performance. Also, there are some significant gaps in the existing literature described in the previous subsection which are mentioned below.
  • Lack of Standardized Metrological Integration: Lack of standardized metrological integration is one of the major aspects in the literature. Although the existing digital twins highlight the product and process, they don’t often define standard measurement protocols, tolerance limits, uncertainty analysis or in-line metrological validation. Their usefulness for industrial quality control is limited by the lack of precise, reproducible measurement integration. On the other hand, the research which emphasised the importance of dimensional features on performance did not distinctly disclose how to measure and maintain the tolerances in a production line. This split creates an absence of a framework that can connect a real-time, dynamic metrological dataset back to the design-stage tolerance models and forecast the impact of deviation on performance.
  • Absence of Dimensional Variation Propagation Models: Existing studies rarely address how multiple dimensional variations propagate across the component features to sub-assemblies, and ultimately, cell level KPIs. In a review based literature study it was claimed that, although current vision systems can detect the defects, they cannot not convey information related to the impact of the defect on the mechanical or electrical performance of the electrode [83]. It suggested that there is an opportunity to explore how the dimensional data can be fed into a digital system that will be able to analyse the consequence of deviations in the cell performance.
  • Limited Focus on Ramp-up Dynamics: Most digital twins and CPS frameworks implicitly assumed stable and steady-state continuous production, limiting their applicability during highly dynamic NPI ramp-up phases, which remains unexplored. Nonetheless, the cause-effect relationships in battery cell production are still poorly understood which make commissioning of machines and plants difficult [79]. The authors asserted that digital twins enable the process mapping in a virtual environment which allows the ramp-up of the plant virtually with low risks. Also, the optimal points can be detected and implemented in reality. The study suggests that the significance and applicability of a digital system is more relevant during NPI.
  • Reactive Approach: The approaches mentioned in the literature appear to be reactive rather than being proactive. The studies didn’t describe any system that can predict the downstream quality failures based on upstream dimensional deviations and can immediately suggest solutions to diminish the errors. Also, the data management and utilization should be done during the design for manufacturing (DFM) phase, not after the production starts. In the conventional method, production-responsible individuals troubleshoot after a defect emerges. But in case of ramp-up, where hundreds of cells are being fabricated in every minute, this approach seems infeasible.
  • Scarcity of ML & AI integration: As ML started to flourish in the manufacturing field since 2014 [84], and modern artificial intelligence (AI) was introduced as a core concept of Industry 4.0 in 2015 [85], those concepts are comparably young in the field of manufacturing metrology. Therefore, there are plenty of opportunities for integrating machine learning (ML) and artificial intelligence (AI) to make the digital system more dependable. It indicates that the capability of the digital systems might be further enhanced if ML & AI models are integrated with those.
  • Missing Closed-Loop Feedback from Metrology to Process Control: Existing digital manufacturing frameworks scarcely translate dimensional measurement data into actionable decision support for process adjustments or manufacturing design revision during production ramp-up. This is the missing link between digital simulation and the physical process. A closed-loop digital system might be an effective solution to bridge the gap between the virtual design intent, real-time measurement, and manufacturing decision-making.

5. Conclusion

The aim of this review-based study was to find the key performance indicators of battery cells, learn how they are influenced by various types of manufacturing factors, and which type of factors are the largest in number. Additionally, it sought to understand the state-of-the-art monitoring and control mechanisms of those manufacturing factors. Through categorization of manufacturing factors identified from the literature, it was found that dimensional features formed the largest group (18 of 46 total factors). Thus, it was concluded that correlation between dimensional features and the battery cell performance has potentiality to become a profound area of study. Also, it appeared that there is a significant gap in quantification of the correlation between dimensional deviation and battery cell performance. Moreover, it can be concluded from this study that there is an opportunity for developing a dimensional metrology digital system capable of amalgamating the design parameters with actual production data and speculate the consequence of deviation from the desired dimension, thereby accelerating the production ramp-up through early quality maturation. The incorporation of ML or AI models would provide further enhancement by enabling data-driven interpretation, prediction and continuous refinement.

Abbreviations

The following abbreviations are used in this manuscript:
AI Artificial Intelligence
BESS Battery Energy Storage System
CAM Cathode Active Material
CB Carbon Black
CPS Cyber-Physical System
DFM Design for Manufacturing
DTw Digital Twin
EKF Extended Kalman Filter
EOL End of Life
EV Electric Vehicle
Gr Graphite
IR Internal Resistance
IT Information Technology
KPI Key Performance Indicator
LCO Lithium Cobalt Oxide
LFP Lithium Iron Phosphate
Li-ion Lithium-ion
LMO Lithium Manganese Oxide
LNO Lithium Nickel Oxide
LTO Lithium Titanate
ML Machine Learning
NASA National Aeronautics and Space Administration
NMC Nickel Manganese Cobalt
NMP N-Methyl-2-pyrrolidone
NPI New Product Introduction
PET Polyethylene Terephthalate
SEI Solid Electrolyte Interphase
SOC State of Charge
SOH State of Health

Author Contributions

“Conceptualization, T.A. and H.G.; methodology, T.A. and L.H.; validation, H.G., L.H. and M.K.; formal analysis, T.A.; investigation, T.A.; resources, H.G. and L.H; data curation, T.A.; writing—original draft preparation, T.A.; writing—review and editing, H.G., L.H., M.K.; visualization, T.A.; supervision, H.G.; project administration, T.A. All authors have read and agreed to the published version of the manuscript.

Funding

This research received no external funding

Institutional Review Board Statement

Not applicable

Data Availability Statement

We encourage all authors of articles published in MDPI journals to share their research data. In this section, please provide details regarding where data supporting reported results can be found, including links to publicly archived datasets analyzed or generated during the study. Where no new data were created, or where data is unavailable due to privacy or ethical restrictions, a statement is still required. Suggested Data Availability Statements are available in section “MDPI Research Data Policies” at https://www.mdpi.com/ethics.

DURC Statement

Current research is limited to metrology and battery cell.

Acknowledgments

ChatGPT was used as an auxiliary tool to summarize the research papers during rapid review before discarding research papers by screening the abstract. The use of generative AI has not compromised the originality of the research nor the ability to: systematically acquire and understand a substantial body of knowledge, gain detailed understanding of applicable techniques for research and advanced academic enquiry, or conceptualise, design and implement a project for the generation of new knowledge. The authors take full responsibility for the content of this review.

Conflicts of Interest

The authors declare no conflicts of interest.

Abbreviations

The following abbreviations are used in this manuscript:

Appendix A. Affecting Factors and associated KPIs

Table A1. Affecting factors and associated KPIs
Table A1. Affecting factors and associated KPIs
Affecting Factor KPIs affected Battery chemistry Factor Type Other Applicable chemistries
Anode-cathode overhang Capacity LFP Dimensional All graphite based anodes [41]
Carbon binder ratio Capacity NMC & LMO Material LFP [86]
Cathode coating thickness Capacity NMC Dimensional LFP [87], LMO [88]
Coating weight Capacity NMC Process LFP [87], LMO [89]
Anode height Capacity NMC Dimensional LFP [90]
Cathode height Capacity NMC Dimensional LFP [90]
Cathode width Capacity NMC Dimensional LFP [90]
Anode width Capacity NMC Dimensional LFP [90]
Cathode material synthesis Capacity LFP, NMC, LMO Process All three
Roll gap Capacity NMC Process None found
Roller temperature Capacity NMC Process None found
Cathode material Price Cost All External All
Labour cost Cost All External All
Production volume Cost All Process All
Scrap rate Cost All Process All
Anode-cathode overhang Cycle Life LFP Dimensional All graphite based anodes [41]
Electrode heterogeneity Cycle life NMC Material LFP [91]
Jelly roll roundness Cycle life LFP Dimensional NMC [92]
SEI formation protocol Cycle life NMC Process LFP [93]
Tab material Cycle life NMC Process LFP [91]
Weld tab thickness Cycle life NMC Dimensional All
Cell diameter Energy NMC Dimensional LFP [94]
Cell height Energy NMC Dimensional LFP [94]
Anode particle size Energy Density LMO External None found
Anode thickness Energy Density LMO Dimensional NMC [95], LFP [96]
Cathode thickness Energy Density LMO Dimensional LFP & NMC (Reverse Effect) [97]
Current collector thickness Energy density LMO Dimensional LFP, NMC [98]
Positive electrode porosity Energy density LCO Material All Li-ion, as stated by [52]
Mass loading Energy density NMC Process LFP [99], LMO [100]
N:P ratio Energy density LCO Dimensional & Chemical LFP & NMC [101], LMO [102]
Nickel content Energy density NMC Material None found
Separator thickness Energy density Various Dimensional LFP [103], NMC [104]
Electrolyte amount Charging capability & Fast-charging Performance NMC Process None found
Mixing intensity Charging capability & Fast-charging Performance NMC Process All Graphite based anodes
Calendering pressure Charging capability & Fast-charging performance NMC Process All graphite based anodes
Terminal cap resistance Internal resistance Didn’t mention External All, as cap resistance doesn’t depend on chemistry
Coating speed Internal resistance Didn’t mention Process All Li-ion batteries
Cathode thickness Internal resistance NMC Dimensional LFP [105]
Mixing quality Internal resistance Didn’t mention Process All, which uses slurry mixing in manufacturing
Active material fraction Power NMC Material None found
Cathode coating thickness Power LMO Dimensional NMC, LFP [106]
Anode thickness Power LMO Dimensional None found
Current collector thickness Power Density LMO Dimensional LFP, NMC [98]
Cathode coating thickness Power density NMC Dimensional LFP [107].
Particle size Power density LMO Material NMC [95]
Separator thickness Power density LMO Dimensional NMC [95]
Electrolyte composition Safety Not specified Material All Li-ions
Metal particle contamination Safety Not specified External All Li-ions
Anode-cathode overhang Safety LFP Dimensional NMC [108], LMO [109]
Tab thickness Safety Not specified Dimensional All Li-ions
Weld penetration depth Safety Not specified Dimensional All Li-ions
Negative electrode porosity Temperature LNO Material LFP [107]
Positive electrode porosity Temperature LNO Material NMC [110], LFP [107]
Cathode coating thickness Temperature LNO Dimensional NMC[111], LFP[112]
Particle size Temperature Graphite Material None found
Tab width Temperature LTO Dimensional All, as it follows Pouillet’s Law of resistance
Nickel content Voltage NMC Material None found
Weld seam width Internal resistance Not specified Dimensional All cells with foil-to-tab join
Weld seam length Internal resistance Not specified Dimensional All cells with foil-to-tab join

References

  1. Amer, M.; Masri, J.; Dababat, A.; Sajjad, U.; Hamid, K. Electric vehicles: Battery technologies, charging standards, AI communications, challenges, and future directions. Energy Convers. Manag. X 2024, 24, 100751. [Google Scholar] [CrossRef]
  2. Manoharan, A.; Chong, J.J.; Choong, Z.J.; Lambert, S.; Kumar Gupta, R.; Chandra, D.; Jain, A.; Rao, A.; Sharma, A. Optimizing lithium-ion battery manufacturing with digitalization and AI-driven frameworks. Int. J. Adv. Manuf. Technol. 2026, 142, 1–37. [Google Scholar] [CrossRef]
  3. Matsumura, N. Practical Battery Design and Control; Artech, 2023; pp. 103–105. [Google Scholar]
  4. Baazouzi, S.; Feistel, N.; Wanner, J.; Landwehr, I.; Fill, A.; Birke, K.P. Design, Properties, and Manufacturing of Cylindrical Li-Ion Battery Cells—A Generic Overview. Batteries 2023, 9. [Google Scholar] [CrossRef]
  5. Liu, Y.; Zhang, R.; Wang, J.; Wang, Y. Current and future lithium-ion battery manufacturing. iScience 2021, 24, 102332. [Google Scholar] [CrossRef]
  6. Örüm Aydin, A.; Zajonz, F.; Günther, T.; Dermenci, K.B.; Berecibar, M.; Urrutia, L. Lithium-Ion Battery Manufacturing: Industrial View on Processing Challenges, Possible Solutions and Recent Advances. Batteries 2023, 9. [Google Scholar] [CrossRef]
  7. Sharmili, N.; Nagi, R.; Wang, P. A review of research in the Li-ion battery production and reverse supply chains. J. Energy Storage 2023, 68, 107622. [Google Scholar] [CrossRef]
  8. Kumar, N.; Pamarthi, V.V.; Das, A. Investigating laser and ultrasonic welding of pouch cell multi-foil current collectors for electric vehicle battery fabrication. Int. J. Adv. Manuf. Technol. 2024, 134, 2497–2511. [Google Scholar] [CrossRef]
  9. Wood, David L., III; Li, J.; An, S.J. Formation Challenges of Lithium-Ion Battery Manufacturing. Joule 2019, 3, 2884–2888. [Google Scholar] [CrossRef]
  10. Xie, Y.; Wang, S.; Zhang, G.; Takyi-Aninakwa, P.; Fernandez, C.; Blaabjerg, F. A review of data-driven whole-life state of health prediction for lithium-ion batteries: Data preprocessing, aging characteristics, algorithms, and future challenges. J. Energy Chem. 2024, 97, 630–649. [Google Scholar] [CrossRef]
  11. Kang, X.; Liu, K.; Mao, J.; Wang, F.; Hu, X. Enhancing lithium metal battery performance with Co3O4 and Co3S4 modified polypropylene separators: Mechanistic insights and electrochemical advancements. J. Energy Storage 2025, 140, 118990. [Google Scholar] [CrossRef]
  12. Yang, N.C.; Chen, W.C. State of health prediction method for battery cells using bidirectional long short-term memory neural network with time-varying filter empirical mode decomposition. J. Power Sources 2025, 656, 238007. [Google Scholar] [CrossRef]
  13. Fischer, M.; Brand, M.J.; Karger, A.; Gomez, M.R.; Rehm, M.; Natterer, J.; Jossen, A. How degradation of lithium-ion batteries impacts capacity fade and resistance increase: A systematic, correlative analysis. J. Power Sources 2025, 656, 237921. [Google Scholar] [CrossRef]
  14. Zhang, J.; Mo, J.; Zhang, G.; Mo, C.; Wu, H.; Jiang, L.; Jiang, W.; Wang, B.; Liu, J.; Peng, K. Impact of innovative cold welding techniques on the thermo-electrochemical performance of battery modules: A thermal simulation model approach. Appl. Therm. Eng. 2025, 278, 127238. [Google Scholar] [CrossRef]
  15. Huang, J.; Long, R.; Ma, L.; Liu, Z.; Liu, W. Thermal and electric inhomogeneity in lithium-ion battery packs. Appl. Therm. Eng. 2025, 269, 126030. [Google Scholar] [CrossRef]
  16. Gilbert Zequera, R.; Rassõlkin, A.; Vaimann, T.; Kallaste, A. Charge Diagnostics and State Estimation of Battery Energy Storage Systems Through Transformer Models. IEEE Access 2025, PP, 1–1. [Google Scholar] [CrossRef]
  17. Wang, X.; Meng, J.; Azib, T. A Comparative Study of Data-Driven Early-Stage End-of-Life Classification Approaches for Lithium-Ion Batteries. Energies 2024, 17. [Google Scholar] [CrossRef]
  18. Li, H.; Chen, C.; Wei, J.; Chen, Z.; Lei, G.; Wu, L. State of Health (SOH) Estimation of Lithium-Ion Batteries Based on ABC-BiGRU. Electronics 2024, 13. [Google Scholar] [CrossRef]
  19. Aizpurua, M.; Garayalde, E.; Lopetegi, I.; Yeregui, J.; Dorronsoro, X.; Iraola, U. Modular BESS Architecture for Enhanced Performance and Extended Lifetime; 09 2024; pp. 1–7. [Google Scholar] [CrossRef]
  20. Zequera, R.A.G.; Rassõlkin, A.; Vaimann, T.; Kallaste, A. Data Science-based Techniques for Modelling and Diagnostics of Battery Cells Based on End-of-Life criteria. In Proceedings of the 2023 International Conference on Electrical Drives and Power Electronics (EDPE), 2023; pp. 1–6. [Google Scholar] [CrossRef]
  21. Roering, P.; Overhoff, G.M.; Liu, K.L.; Winter, M.; Brunklaus, G. External Pressure in Polymer-Based Lithium Metal Batteries: An Often-Neglected Criterion When Evaluating Cycling Performance? ACS Appl. Mater. Interfaces 2024, 16, 21932–21942. [Google Scholar] [CrossRef] [PubMed]
  22. Hua, J.; Vie, P.J.; Wind, J. Methods for faster estimation of the entropy profile of a lithium-ion battery: A comparison of accelerated potentiometry and the estimation of entropy through thermal signatures. Electrochimica Acta 2025, 509, 145289. [Google Scholar] [CrossRef]
  23. Gilbert Zequera, R.A.; Rjabtšikov, V.; Rassõlkin, A.; Vaimann, T.; Kallaste, A. Deep Learning Methodology for Charging Management Applications in Battery Cells Based on Neural Networks. IEEE Trans. Intell. Veh. 2025, 10, 668–682. [Google Scholar] [CrossRef]
  24. Huemiller, E.; McGovern, M.; Du, X.; Salvador, J.; Wagner, S.; Collin, W. Industrial EV Battery Performance Evaluation: A Review From the Instrumentation Perspective. IEEE Open J. Instrum. Meas. 2025, 4, 1–13. [Google Scholar] [CrossRef]
  25. Carnevali, A.; Palacin, M.R.; Grey, C.P.; Franco, A.A. VOLTA: A tool for battery screening bridging the gap between virtual electrode materials and practical applications. Energy Storage Mater. 2024, 67, 103254. [Google Scholar] [CrossRef]
  26. Voicila, I.T.; Seritan, G.C.; Enache, B.A.; Stanculescu, M.; Porumb, R.F. Design and implementation of a multi-battery, multi-chemistry state of health screening system; 06 2023; pp. 1–4. [Google Scholar] [CrossRef]
  27. Plumeyer, J.F.; Moesle, F.; Wolf, S.; Born, H.; Heimes, H.H.; Kampker, A. Optimisation of Solid-State Batteries: A Modelling Approach to Battery Design. Batteries 2025, 11. [Google Scholar] [CrossRef]
  28. Pegel, H.; Jany, L.; Sauer, D.U. Pareto-Optimal Design of Automotive Battery Systems with Tabless Cylindrical Lithium-Ion Cells: Resolving the Trade-Off Between Energy, Performance, Weight, and Cost for Variable Vehicle Requirements. Energy Technol. 2025, 13, 2401479. Available online: https://onlinelibrary.wiley.com/doi/pdf/10.1002/ente.202401479. [CrossRef]
  29. Muñoz-Torrero, D.; Santana Santos, C.; García-Quismondo, E.; Dieckhöfer, S.; Erichsen, T.; Palma, J.; Schuhmann, W.; Ventosa, E. The redox mediated – scanning droplet cell system for evaluation of the solid electrolyte interphase in Li-ion batteries. RSC Adv. 2023, 13, 15521–15530. [Google Scholar] [CrossRef] [PubMed]
  30. Xiao, J.; Sun, J.; Song, W.; Zhang, X.; Li, X.; Xie, H.; Lu, Z.; Fujishige, M.; Endo, M.; Niu, J.; et al. Fast-charging graphite-based anode enabled by gradient silicon: from mechanism revelation to electrode design. Energy Storage Mater. 2025, 78, 104280. [Google Scholar] [CrossRef]
  31. Çarkıt, T.; Alçı, M. Investigation of Voc and SoH on Li-ion batteries with an electrical equivalent circuit model using optimization algorithms. Electr. Eng. 2024, 106, 1781–1792. [Google Scholar] [CrossRef]
  32. Jin, L.; Kazemi, M.; Comodi, G.; Papadimitriou, C. Assessing battery degradation as a key performance indicator for multi-objective optimization of multi-carrier energy systems. Appl. Energy 2024, 361, 122925. [Google Scholar] [CrossRef]
  33. Li, M.; Hong, J.; Shen, Y.; Ma, F.; Liang, F.; Zhang, L.; Pei, J.; Qiu, Y.; Yang, J.; Xu, Q.; et al. Research on voltage inconsistency diagnosis of power battery based on PSO-VMD-improved local outlier factor. Energy 2025, 333, 137442. [Google Scholar] [CrossRef]
  34. Koech, A.K.; Mwandila, G.; Mulolani, F.; Mwaanga, P. Lithium-ion battery fundamentals and exploration of cathode materials: A review. South Afr. J. Chem. Eng. 2024, 50, 321–339. [Google Scholar] [CrossRef]
  35. Schindler, M.; Sturm, J.; Ludwig, S.; Schmitt, J.; Jossen, A. Evolution of initial cell-to-cell variations during a three-year production cycle. eTransportation 2021, 8, 100102. [Google Scholar] [CrossRef]
  36. Broad, R.; Fly, A. Influence of geometrical manufacturing tolerances on lithium-ion battery performance. Int. J. Energy Res. 2022, 46, 23824–23838. Available online: https://onlinelibrary.wiley.com/doi/pdf/10.1002/er.8680. [CrossRef]
  37. Faraji Niri, M.; Apachitei, G.; Lain, M.; Copley, M.; Marco, J. The Impact of Calendering Process Variables on the Impedance and Capacity Fade of Lithium-Ion Cells: An Explainable Machine Learning Approach. Energy Technol. 2022, 10, 2200893. Available online: https://onlinelibrary.wiley.com/doi/pdf/10.1002/ente.202200893. [CrossRef]
  38. Lenze, G.; Laue, V.; Krewer, U. Time-Efficient Reparameterization and Simulation of Manufacturing Impacts on Performance of Lithium-Ion-Batteries. J. Electrochem. Soc. 2019, 166, A2950. [Google Scholar] [CrossRef]
  39. Koech, A.K.; Mwandila, G.; Mulolani, F. A review of improvements on electric vehicle battery. Heliyon 2024, 10. [Google Scholar] [CrossRef] [PubMed]
  40. Schulze, M.C.; Rodrigues, M.T.F.; McBrayer, J.D.; Abraham, D.P.; Apblett, C.A.; Bloom, I.; Chen, Z.; Colclasure, A.M.; Dunlop, A.R.; Fang, C.; et al. Critical Evaluation of Potentiostatic Holds as Accelerated Predictors of Capacity Fade during Calendar Aging. J. Electrochem. Soc. 2022, 169, 050531. [Google Scholar] [CrossRef]
  41. Lewerenz, M.; Münnix, J.; Schmalstieg, J.; Käbitz, S.; Knips, M.; Sauer, D.U. Systematic aging of commercial LiFePO4|Graphite cylindrical cells including a theory explaining rise of capacity during aging. J. Power Sources 2017, 345, 254–263. [Google Scholar] [CrossRef]
  42. Dammala, P.K.; Dermenci, K.B.; Kathribail, A.R.; Yadav, P.; Van Mierlo, J.; Berecibar, M. A critical review of future aspects of digitalization next generation Li-ion batteries manufacturing process. J. Energy Storage 2023, 74, 109209. [Google Scholar] [CrossRef]
  43. Spiers, D. Chapter II-2-B - Batteries in PV Systems. In McEvoy’s Handbook of Photovoltaics (Third Edition), Third Edition ed.; Kalogirou, S.A., Ed.; Academic Press, 2018; pp. 789–843. [Google Scholar] [CrossRef]
  44. Weng, A.; Mohtat, P.; Attia, P.M.; Sulzer, V.; Lee, S.; Less, G.; Stefanopoulou, A. Predicting the impact of formation protocols on battery lifetime immediately after manufacturing. Joule 2021, 5, 2971–2992. [Google Scholar] [CrossRef]
  45. Waldmann, T.; Scurtu, R.G.; Brändle, D.; Wohlfahrt-Mehrens, M. Effects of Tab Design in 21700 Li-Ion Cells: Improvements of Cell Impedance, Rate Capability, and Cycling Aging. Energy Technol. 2023, 11, 2200583. Available online: https://onlinelibrary.wiley.com/doi/pdf/10.1002/ente.202200583. [CrossRef]
  46. Kim, M.; Kim, I.; Kim, J.; Choi, J.W. Lifetime Prediction of Lithium Ion Batteries by Using the Heterogeneity of Graphite Anodes. ACS Energy Lett. 2023, 8, 2946–2953. [Google Scholar] [CrossRef]
  47. Sieg, J.; Schmid, A.U.; Rau, L.; Gesterkamp, A.; Storch, M.; Spier, B.; Birke, K.P.; Sauer, D.U. Fast-charging capability of lithium-ion cells: Influence of electrode aging and electrolyte consumption. Appl. Energy 2022, 305, 117747. [Google Scholar] [CrossRef]
  48. Huber, K.; Adam, A.; Grießl, D.; Kwade, A. Understanding slurry mixing effects on the fast charging capability of lithium-ion battery cells: Methodology and case study. J. Power Sources 2022, 536, 231455. [Google Scholar] [CrossRef]
  49. Strzelczyk, N.; Gottschalk, L.; Müller, J.; Kwade, A. The Influence of Calendering on the Fast Charging Performance and Lithium Plating of Hard Carbon Blend Anodes. Energy Technol. 2023, 11, 2200865. [Google Scholar] [CrossRef]
  50. Orangi, S.; Strømman, A.H. A Techno-Economic Model for Benchmarking the Production Cost of Lithium-Ion Battery Cells. Batteries 2022, 8. [Google Scholar] [CrossRef]
  51. Mauler, L.; Duffner, F.; Leker, J. Economies of scale in battery cell manufacturing: The impact of material and process innovations. Appl. Energy 2021, 286, 116499. [Google Scholar] [CrossRef]
  52. Yourey, W. Cell Design Considerations and Impact on Energy Density—A Practical Approach to EV Cell Design. World Electr. Veh. J. 2023, 14. [Google Scholar] [CrossRef]
  53. Park, J.; Yoo, D.; Moon, J.; Yoon, J.; Park, J.; Lee, S.; Lee, D.; Kim, C. Reliability-Based Robust Design Optimization of Lithium-Ion Battery Cells for Maximizing the Energy Density by Increasing Reliability and Robustness. Energies 2021, 14. [Google Scholar] [CrossRef]
  54. Schmidt, O.; Thomitzek, M.; Röder, F.; Thiede, S.; Herrmann, C.; Krewer, U. Modeling the Impact of Manufacturing Uncertainties on Lithium-Ion Batteries. J. Electrochem. Soc. 2020, 167, 060501. [Google Scholar] [CrossRef]
  55. Khan, F.N.U.; Rasul, M.G.; Sayem, A.; Mandal, N. Maximizing energy density of lithium-ion batteries for electric vehicles: A critical review. Energy Rep. Proc. 2022 7th Int. Conf. Renew. Energy Conserv. 2023, 9, 11–21. [Google Scholar] [CrossRef]
  56. Cui, S.; Sun, J.; Liu, Z.; Sheng, J.; Chen, Y.; Yu, H.; Zhang, D. Study on internal resistance of Li-ion power battery. J. Intell. Manuf. Spec. Equip. 2025, 6, 54–66. Available online: https://www.emerald.com/jimse/article-pdf/6/1/54/10059527/jimse-11-2024-0034.pdf. [CrossRef]
  57. Kisu, K.; Aoyagi, S.; Nagatomo, H.; Iwama, E.; Reid, M.T.H.; Naoi, W.; Naoi, K. Internal resistance mapping preparation to optimize electrode thickness and density using symmetric cell for high-performance lithium-ion batteries and capacitors. J. Power Sources 2018, 396, 207–212. [Google Scholar] [CrossRef]
  58. Asirvatham, M.C.; Nakhanivej, P.; Perry-French, V.A.; Altaf, E.F.; Loveridge, M.J.; Pathan, T.S.; McLaggan, J.D. Architectural Evolution and Advanced Joining Techniques in High-Energy-Density Cylindrical Li-Ion Cells. Batteries 2026, 12. [Google Scholar] [CrossRef]
  59. Grabmann, S.; Bernauer, C.; Wach, L.; Leeb, M.; Zaeh, M.F. A method for the reproducible and accurate determination of electrical resistances based on multi-layer joints in lithium-ion batteries. Appl. Energy 2023, 349, 121613. [Google Scholar] [CrossRef]
  60. Kang, J.; Lee, S.; Choi, Y.C.; Myeong, S.; Park, S.; Kang, H.S.; Shin, J.; Lee, J.W.; You, M.; Shin, S.S.; et al. Atomic-Scale Tailoring of Ni-Rich Cathodes for the Development of Commercial Li-Ion Batteries: From Laboratory to Market. Adv. Sci. n/a, e15521. Available online: https://advanced.onlinelibrary.wiley.com/doi/pdf/10.1002/advs.202515521. [CrossRef] [PubMed]
  61. Duquesnoy, M.; Liu, C.; Kumar, V.; Ayerbe, E.; Franco, A.A. Toward high-performance energy and power battery cells with machine learning-based optimization of electrode manufacturing. J. Power Sources 2024, 590, 233674. [Google Scholar] [CrossRef]
  62. Zhao, R.; Liu, J.; Gu, J. The effects of electrode thickness on the electrochemical and thermal characteristics of lithium ion battery. Appl. Energy 2015, 139, 220–229. [Google Scholar] [CrossRef]
  63. Ilyas, A.; Kashif, S.A.; Saqib, M.A.; Asad, M.M. Wave electrical energy systems: Implementation, challenges and environmental issues. Renew. Sustain. Energy Rev. 2014, 40, 260–268. [Google Scholar] [CrossRef]
  64. Xie, W.; Zhang, Z.; Gao, X. Understanding the limitations of thick electrodes on the rate capability of high-energy density lithium-ion batteries. Electrochimica Acta 2024, 493, 144396. [Google Scholar] [CrossRef]
  65. Kim, C., Perea, A., Rozon, D., Dubé, J., Eds.; Quantitative Measurement of the Safety Performance of Li-Ion Batteries. ECS Meet. Abstr. 2023, MA2023-01, 616. [Google Scholar] [CrossRef]
  66. Attia, P.M.; Moch, E.; Herring, P.K. Challenges and opportunities for high-quality battery production at scale. Nat. Commun. 2025, 16, 611. [Google Scholar] [CrossRef] [PubMed]
  67. Yao, X.Y.; Pecht, M.G. Tab Design and Failures in Cylindrical Li-ion Batteries. IEEE Access 2019, 7, 24082–24095. [Google Scholar] [CrossRef]
  68. Botte, G.G.; Johnson, B.A.; White, R.E. Influence of Some Design Variables on the Thermal Behavior of a Lithium-Ion Cell. J. Electrochem. Soc. 1999, 146, 914. [Google Scholar] [CrossRef]
  69. Goutam, S.; Timmermans, J.M.; Omar, N.; Bossche, P.V.d.; Van Mierlo, J. Comparative Study of Surface Temperature Behavior of Commercial Li-Ion Pouch Cells of Different Chemistries and Capacities by Infrared Thermography. Energies 2015, 8, 8175–8192. [Google Scholar] [CrossRef]
  70. Chen, C.F.; Verma, A.; Mukherjee, P.P. Probing the Role of Electrode Microstructure in the Lithium-Ion Battery Thermal Behavior. J. Electrochem. Soc. 2017, 164, E3146. [Google Scholar] [CrossRef]
  71. Tang, K.; Luo, B.; Chen, D.; Wang, C.; Chen, L.; Li, F.; Cao, Y.; Wang, C. The State of Health Estimation of Lithium-Ion Batteries: A Review of Health Indicators, Estimation Methods, Development Trends and Challenges. World Electr. Veh. J. 2025, 16. [Google Scholar] [CrossRef]
  72. Xie, J.; Wei, X.; Bo, X.; Zhang, P.; Chen, P.; Hao, W.; Yuan, M. State of Charge Estimation of Lithium-Ion Battery Based on Extended Kalman Filter Algorithm. Front. Energy Res. 2023, 11, 1180881. [Google Scholar] [CrossRef]
  73. Wlazlak, P.; Hussmo, D.; Säfsten, K. Integration Across Knowledge Boundaries During New Product Introduction. In Transdisciplinary Engineering for Resilience: Responding to System Disruptions; Newnes, L., et al., Eds.; IOS Press, 2021; pp. 405–414. [Google Scholar] [CrossRef]
  74. Säfsten, K.; Bellgran, M. From System Solution to Production System in Operation. In Production Development: Design and Operation of Production Systems; Springer London: London, 2010; pp. 231–254. [Google Scholar] [CrossRef]
  75. Leithoff, R.; Dilger, N.; Duckhorn, F.; Blume, S.; Lembcke, D.; Tschöpe, C.; Herrmann, C.; Dröder, K. Inline Monitoring of Battery Electrode Lamination Processes Based on Acoustic Measurements. Batteries 2021, 7. [Google Scholar] [CrossRef]
  76. Terwiesch, C.; E. Bohn, R. Learning and process improvement during production ramp-up. Int. J. Prod. Econ. 2001, 70, 1–19. [Google Scholar] [CrossRef]
  77. Thelen, A.; Zhang, X.; Fink, O.; Lu, Y.; Ghosh, S.; Youn, B.D.; Todd, M.D.; Mahadevan, S.; Hu, C.; Hu, Z. A comprehensive review of digital twin — part 1: modeling and twinning enabling technologies. Struct. Multidiscip. Optim. 2022, 65, 354. [Google Scholar] [CrossRef]
  78. Tao, F.; Qi, Q.; Wang, L.; Nee, A. Digital Twins and Cyber–Physical Systems toward Smart Manufacturing and Industry 4.0: Correlation and Comparison. Engineering 2019, 5, 653–661. [Google Scholar] [CrossRef]
  79. Husseini, K.; Schmidgruber, N.; Weinmann, H.; Maibaum, K.; Ruhland, J.; Fleischer, J. Development of a Digital Twin for Improved Ramp-Up Processes in the Context of Li-Ion-Battery-Cell-Stack-Formation. Procedia CIRP 9th CIRP Conference on Assembly Technology and Systems, 2022; 106, pp. 27–32. [Google Scholar] [CrossRef]
  80. Turetskyy, A.; Wessel, J.; Herrmann, C.; Thiede, S. Data-driven cyber-physical System for Quality Gates in Lithium-ion Battery Cell Manufacturing. Procedia CIRP 53rd CIRP Conference on Manufacturing Systems 2020, 2020; 93, pp. 168–173. [Google Scholar] [CrossRef]
  81. Kies, A.D.; Krauß, J.; Schmetz, A.; Schmitt, R.H.; Brecher, C. Interaction of Digital Twins in a Sustainable Battery Cell Production. Procedia CIRP Leading manufacturing systems transformation – Proceedings of the 55th CIRP Conference on Manufacturing Systems 2022 2022, 107, 1216–1220. [Google Scholar] [CrossRef]
  82. Kampker, A.; Heimes, H.H.; Dorn, B.; Clever, H.; Ludwigs, R.; Li, R.; Drescher, M. Concept for Digital Product Twins in Battery Cell Production. World Electr. Veh. J. 2023, 14. [Google Scholar] [CrossRef]
  83. McGovern, M.E.; Bruder, D.D.; Huemiller, E.D.; Rinker, T.J.; Bracey, J.T.; Sekol, R.C.; Abell, J.A. A review of research needs in nondestructive evaluation for quality verification in electric vehicle lithium-ion battery cell manufacturing. J. Power Sources 2023, 561, 232742. [Google Scholar] [CrossRef]
  84. Kausik, A.K.; Rashid, A.B.; Baki, R.F.; Jannat Maktum, M.M. Machine learning algorithms for manufacturing quality assurance: A systematic review of performance metrics and applications. Array 2025, 26, 100393. [Google Scholar] [CrossRef]
  85. Majstorovic, V.; Djurdjanovic, D.; Stojadinovic, S. Development and application of artificial intelligence in manufacturing systems – one approach. Procedia CIRP 58th CIRP Conference on Manufacturing Systems 2025, 2025; 134, pp. 753–758. [Google Scholar] [CrossRef]
  86. Konda, K.; Jacob, M.S.; Seth, J.R.; Juvekar, V.A.; Gopalan, R.; Moodakare, S.B. Capacity degradation of lithium-ion cell: The role of free carbon black content in the slurry and drying induced cracks in LiFePO4 electrode. J. Energy Storage 2023, 74, 109477. [Google Scholar] [CrossRef]
  87. de la Torre-Gamarra, C.; Sotomayor, M.E.; Sanchez, J.Y.; Levenfeld, B.; Várez, A.; Laïk, B.; Pereira-Ramos, J.P. High mass loading additive-free LiFePO4 cathodes with 500 μm thickness for high areal capacity Li-ion batteries. J. Power Sources 2020, 458, 228033. [Google Scholar] [CrossRef]
  88. Hamankiewicz, B.; Michalska, M.; Krajewski, M.; Ziolkowska, D.; Lipinska, L.; Korona, K.; Kaminska, M.; Czerwinski, A. The effect of electrode thickness on electrochemical performance of LiMn2O4 cathode synthesized by modified sol–gel method. Solid State Ionics Solid State Ionics 19 Proceedings of the 19th International Conference on Solid State Ionics 2014, 262, 9–13. [Google Scholar] [CrossRef]
  89. Guo, Y.; Li, X.; Wang, Z.; Wang, J.; Guo, H.; Yan, G. Free-standing ultrathick LiMn2O4@single-wall carbon nanotubes electrode with high areal capacity. J. Energy Chem. 2022, 73, 452–459. [Google Scholar] [CrossRef]
  90. Siegel, J.B.; Stefanopoulou, A.G.; Hagans, P.; Ding, Y.; Gorsich, D. Expansion of Lithium Ion Pouch Cell Batteries: Observations from Neutron Imaging. J. Electrochem. Soc. 2013, 160, A1031–A1038. [Google Scholar] [CrossRef]
  91. Petz, D.; Mühlbauer, M.; Baran, V.; Kornmeier, J.R.; Schökel, A.; Pirling, T.; Müller-Buschbaum, P.; Senyshyn, A. Influence of current tabs on performance and aging of multi-tab 26650-type LFP lithium-ion batteries. J. Energy Storage 2025, 115, 115911. [Google Scholar] [CrossRef]
  92. Pfrang, A.; Kersys, A.; Kriston, A.; Sauer, D.; Rahe, C.; Käbitz, S.; Figgemeier, E. Long-term cycling induced jelly roll deformation in commercial 18650 cells. J. Power Sources 2018, 392, 168–175. [Google Scholar] [CrossRef]
  93. Moretti, A.; Sharova, V.; Carvalho, D.V.; Boulineau, A.; Porcher, W.; de Meatza, I.; Passerini, S. A Comparison of Formation Methods for Graphite//LiFePO4 Cells. Batter. Supercaps 2019, 2, 240–247. Available online: https://chemistry-europe.onlinelibrary.wiley.com/doi/pdf/10.1002/batt.201800109. [CrossRef]
  94. Shukla, V.; Mishra, A.; Sure, J.; Ghosh, S.; Tewari, R.P. Size-dependent failure behavior of commercially available lithium-iron phosphate battery under mechanical abuse. Process Saf. Prog. 2023, 42, 674–685. Available online: https://aiche.onlinelibrary.wiley.com/doi/pdf/10.1002/prs.12501. [CrossRef]
  95. Singh, M.; Kaiser, J.; Hahn, H. Effect of Porosity on the Thick Electrodes for High Energy Density Lithium Ion Batteries for Stationary Applications. Batteries 2016, 2. [Google Scholar] [CrossRef]
  96. Yu, S.; Kim, S.; Kim, T.Y.; Nam, J.H.; Cho, W.I. Model Prediction and Experiments for the Electrode Design Optimization of LiFePO4/Graphite Electrodes in High Capacity Lithium-ion Batteries. Bull. Korean Chem. Soc. 2013, 34, 79–88. [Google Scholar] [CrossRef]
  97. Khan, F.N.; Rasul, M.G.; Sayem, A.; Mandal, N.K. A computational analysis of effects of electrode thickness on the energy density of lithium-ion batteries. Energy 2024, 288, 129774. [Google Scholar] [CrossRef]
  98. Zhu, P.; Gastol, D.; Marshall, J.; Sommerville, R.; Goodship, V.; Kendrick, E. A review of current collectors for lithium-ion batteries. J. Power Sources 2021, 485, 229321. [Google Scholar] [CrossRef]
  99. Franke-Lang, R.; Kowal, J. Electrochemical Model-Based Investigation of Thick LiFePO4 Electrode Design Parameters. Modelling 2021, 2, 259–287. [Google Scholar] [CrossRef]
  100. Airoldi, L.; Anselmi-Tamburini, U.; Vigani, B.; Rossi, S.; Mustarelli, P.; Quartarone, E. Additive Manufacturing of Aqueous-Processed LiMn2O4 Thick Electrodes for High-Energy-Density Lithium-Ion Batteries. Batter. Supercaps 2020, 3, 1040–1050. Available online: https://chemistry-europe.onlinelibrary.wiley.com/doi/pdf/10.1002/batt.202000058. [CrossRef]
  101. Niri, M.F.; Apachitei, G.; Lain, M.; Copley, M.; Marco, J. Machine learning for investigating the relative importance of electrodes’ N:P areal capacity ratio in the manufacturing of lithium-ion battery cells. J. Power Sources 2022, 549, 232124. [Google Scholar] [CrossRef]
  102. Jeon, Y.; Noh, H.K.; Song, H.K. A Lithium-ion Battery Using Partially Lithiated Graphite Anode and Amphi-redox LiMn2O4 Cathode. Sci. Rep. 2017, 7, 14879. [Google Scholar] [CrossRef] [PubMed]
  103. Li, Y.; Tan, Z. Effects of a Separator on the Electrochemical and Thermal Performances of Lithium-Ion Batteries: A Numerical Study. Energy Fuels 2020, 34, 14915–14923. [Google Scholar] [CrossRef]
  104. Chang, Z.; Yang, H.; Pan, A.; He, P.; Zhou, H. An improved 9 micron thick separator for a 350 Wh/kg lithium metal rechargeable pouch cell. Nat. Commun. 2022, 13, 6788. [Google Scholar] [CrossRef] [PubMed]
  105. Jeong, J.; Lee, H.; Choi, J.; Ryou, M.H.; Lee, Y.M. Effect of LiFePO4 cathode density and thickness on electrochemical performance of lithium metal polymer batteries prepared by in situ thermal polymerization. Electrochimica Acta 2015, 154, 149–156. [Google Scholar] [CrossRef]
  106. Zheng, H.; Li, J.; Song, X.; Liu, G.; Battaglia, V.S. A comprehensive understanding of electrode thickness effects on the electrochemical performances of Li-ion battery cathodes. Electrochimica Acta 2012, 71, 258–265. [Google Scholar] [CrossRef]
  107. Hosseinzadeh, E.; Marco, J.; Jennings, P. The impact of multi-layered porosity distribution on the performance of a lithium ion battery. Appl. Math. Model. 2018, 61, 107–123. [Google Scholar] [CrossRef]
  108. Cao, C.; Steinrück, H.G.; Paul, P.P.; Dunlop, A.R. Conformal Pressure and Fast-Charging Li-Ion Batteries. J. Electrochem. Soc. 2022, 169, 040540. [Google Scholar] [CrossRef]
  109. Grimsmann, F.; Gerbert, T.; Brauchle, F.; Gruhle, A.; Parisi, J.; Knipper, M. Hysteresis and current dependence of the graphite anode color in a lithium-ion cell and analysis of lithium plating at the cell edge. J. Energy Storage 2018, 15, 17–22. [Google Scholar] [CrossRef]
  110. Chen, C.F.; Verma, A.; Mukherjee, P. Probing the Role of Electrode Microstructure in the Lithium-Ion Battery Thermal Behavior. J. Electrochem. Soc. 2017, 164, E3146–E3158. [Google Scholar] [CrossRef]
  111. Kubarkov, A.V.; Babkin, A.V.; Drozhzhin, O.A.; Stevenson, K.J.; Antipov, E.V.; Sergeyev, V.G. Engendering High Energy Density LiFePO4 Electrodes with Morphological and Compositional Tuning. Nanomaterials 2023, 13. [Google Scholar] [CrossRef] [PubMed]
  112. AL-NEAMA, A.; THOMPSON, H. The impact of electrode design parameters on the thermal behavior of a lithium-ion battery. J. Therm. Eng. 2025, 11, 1094–1119. [Google Scholar] [CrossRef]
Figure 1. Rapid Review diagram of the review steps.
Figure 1. Rapid Review diagram of the review steps.
Preprints 245191 g001
Figure 2. Distribution of manufacturing factors affecting KPIs.
Figure 2. Distribution of manufacturing factors affecting KPIs.
Preprints 245191 g002
Table 1. Studies excluded after full-text review with reasons.
Table 1. Studies excluded after full-text review with reasons.
Study Reasons for Exclusion
[11] Didn’t address any parameters as KPI of batteries.
[12] Didn’t mention any KPI.
[13] About correlation between internal resistance (IR) and capacity fade. Did not recognise any KPI.
[14] Focused on pack performance rather than cell performance.
[15] Mentioned some KPIs of thermal and electrical inhomogeneity, not battery cell.
[16] Mentioned about KPIs of battery energy storage system (BESS), not cell.
[17] Based on machine learning (ML) model for forecasting early-life degradation.
[18] Discussed about ML model development. Didn’t address any parameters as KPIs.
[19] Although introduced a new KPI, it is applicable for analysing the modular connection of batteries.
[20] Based on ML models of BESS. Didn’t mention anything about cell KPI.
[21] Discussed about KPI of cell of solid electrolyte chemistry.
Table 2. Key performance indicators (KPIs) and the studies where it is mentioned.
Table 2. Key performance indicators (KPIs) and the studies where it is mentioned.
KPI name Reported in
Capacity [22,23,24,25,26]
Charging capability [27]
Cost [27,28]
Cycle life [22,27,29]
Energy [28]
Energy density [27]
Fast-charging performance [28,30]
Internal resistance [26,27]
Open-circuit voltage (OCV) [31]
Power [22]
Power density [27,29]
Safety [22,27]
State of charge (SOC) [23]
State of health (SOH) [26,31,32]
Temperature [24]
Voltage [23,25,33]
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.
Copyright: This open access article is published under a Creative Commons CC BY 4.0 license, which permit the free download, distribution, and reuse, provided that the author and preprint are cited in any reuse.