Preprint
Article

This version is not peer-reviewed.

Prediction of Deep Neural Network for TCAD Analysis of Degradation Induced by Near-Interface Displacement Defects in 4H-SiC MOSFETs

A peer-reviewed article of this preprint also exists.

Submitted:

16 October 2026

Posted:

19 October 2026

You are already at the latest version

Abstract
Silicon carbide (SiC) devices used in space and nuclear environments are exposed to radiation that creates displacement defects, and the effect of these defects near the gate oxide/SiC interface has not been analyzed systematically. This paper analyzes the effects of displacement defects (DDs) near this interface in a 4H-SiC metal-oxide-semiconductor field-effect transistor (MOSFET) on the threshold voltage (Vth), transconductance (gm), and on-current (Ion) using technology computer-aided design (TCAD) simulation, and builds deep neural network (DNN) models that predict these effects. The DDs were modeled as acceptor-like traps, and their energy level, concentration, depth, lateral position, and distribution width were varied. The degradation was largest when the traps were located in the channel and at the edge of the junction field-effect transistor (JFET) region, and the depth mattered little as long as the trap region reached the interface. In addition, shallow-level traps reduced Ion without shifting Vth, whereas deep-level traps also increased Vth. All three DNN models for Vth, gm, and Ion reproduced the TCAD simulation results with high accuracy. Because the trained DNNs can rapidly predict the degradation for trap conditions not used in training within the valid range, they can be used for radiation reliability assessment of SiC MOSFETs.
Keywords: 
;  ;  ;  

1. Introduction

4H-SiC is a semiconductor with a wide bandgap of 3.26 eV and a breakdown field about ten times that of Si. For the same breakdown voltage, the drift region can be designed to be thinner and more heavily doped, enabling power devices with a low on-resistance (Ron) [1,2]. Because SiC metal-oxide-semiconductor field-effect transistors (MOSFETs) are applied in space and terrestrial environments such as satellite systems and nuclear power plants, radiation can affect the device characteristics, and a quantitative evaluation of radiation-induced degradation is required [3,4].
Displacement defects (DDs), one of the effects of radiation on semiconductor devices, are permanent defects formed inside a semiconductor when incident particles collide with lattice atoms and displace them from their lattice sites [5]. In 4H-SiC, DDs can form deep acceptor levels, and in n-type regions these levels capture electrons, become negatively charged, and compensate donors, thereby reducing the effective carrier concentration [6,7]. In particular, defects formed near the interface between the gate oxide and SiC can modulate the current path under the gate and reduce the on-current (Ion) [8]. The effects of DDs vary depending on various factors, such as position, energy level, concentration, and distribution width. Therefore, to evaluate the radiation reliability with respect to DDs, it is necessary to analyze the degradation of the threshold voltage (Vth), transconductance (gm), and Ion by considering these factors in combination, rather than examining each variable individually.
Because it is difficult to locally control defects with a desired concentration and energy level at a specific position, technology computer-aided design (TCAD) simulation is used to analyze the effect of each defect variable [9]. A previous related study varied the defect position within a SiC MOSFET and focused on the device-scale position dependence [8]. This study focuses on the near-interface region itself and analyzes the degradation by combining the lateral position of the defects with their depth from the interface, distribution width, concentration, and energy level.
A detailed analysis of the effects of these near-interface defects requires varying the depth and distribution width of the defects on the nanometer scale and combining them with the concentration and energy level to consider various conditions. However, TCAD simulation requires minutes to hours of computation per condition, making an exhaustive search of thousands or more variable combinations difficult. Therefore, a model that learns a dataset generated by TCAD simulation and instantly predicts device characteristics from the input variables is needed [10,11], and we use a deep neural network (DNN), which can learn the nonlinear relationship between inputs and outputs without a separate physical model.
In this study, DDs in the form of acceptor-like traps are placed near the gate oxide interface of a 4H-SiC MOSFET using TCAD simulation, and a dataset of 11,200 conditions is generated by combining five trap variables: energy level, concentration, depth from the interface, lateral position, and spatial distribution width. We analyze the effects of the DDs, which vary with these variables, on Vth, gm, and Ion and present a physical interpretation. On this basis, we define the valid dataset range, train DNNs, and evaluate their predictions using the coefficient of determination R2 and the mean absolute error (MAE).

2. TCAD Simulation and Dataset

2.1. Device Structure and Simulation Conditions

Figure 1 shows the TCAD simulation structure of a planar 4H-SiC n-channel MOSFET, modeled as a half-cell with a width of 5 μm. The n- drift layer, 10 μm thick with a doping concentration of 5×1015 cm-3 lies on an n⁺ substrate (1×1019 cm-3); the n-type drift region in direct contact with the gate oxide surface constitutes the junction field-effect transistor (JFET) region. The lateral coordinate Y is defined with the center of the cell as the origin, and the depth coordinate X is defined with the SiC surface as the origin; as Y increases, the JFET region, channel, and n⁺ source appear.
The simulations were performed with the two-dimensional drift-diffusion method using Synopsys Sentaurus TCAD simulation [12]. Fermi-Dirac statistics were used for the carrier distribution [13], and the Shockley-Read-Hall model with doping and temperature dependence and the Auger model were applied for recombination. The mobility model included doping concentration dependence, high-field saturation, and mobility degradation due to the electric field normal to the interface, and the mobility anisotropy according to the 4H-SiC crystal direction was also considered [14].
The lattice temperature was fixed at 300 K. Because a two-dimensional TCAD simulation calculates the current per 1 μm of device width, the half-cell current was multiplied by 5×105. This accounts for the third dimension of the MOSFET and reproduces the current that an actual device would carry; it corresponds to 5×105 half-cells connected in parallel. The ID-VGS transfer curves were obtained by sweeping VGS from 0 V to 10 V at VDS=10 V, and Vth was determined by the constant-current method, defined as the VGS at which ID reaches the reference current Io=1 mA. gm was extracted as the maximum slope obtained by dividing the change in ID by the change in VGS between two adjacent points, and Ion is the drain current at VGS=VDS=10 V. Under conditions where ID did not reach 1 mA within the sweep range, Vth cannot be extracted by the constant-current method, so values extrapolated beyond the sweep range were not used as Vth.

2.2. DD Modeling and Dataset

The DDs were implemented as acceptor-like traps in the SiC bulk. Because an acceptor-like trap is negatively charged when it captures an electron and neutral when it is empty, in n-type regions where the Fermi level is above the trap level, the traps capture electrons, become negatively charged, and compensate donors [7,12]. The traps were placed uniformly with a concentration Nt within a range of ±σ in each direction from the center (X, Y), and the portion extending outside the SiC surface was excluded. Therefore, σ is the half-width of the trap region, and the total amount of traps depends on Nt and the actual size of the trap region inside the SiC. The energy level is the depth Ec-Et measured from the bottom of the conduction band. As shown in Table 1, simulations were performed for 5×8×8×7×5=11,200 conditions through a full-factorial combination of five energy levels, eight concentrations, eight depths, seven lateral positions, and five distribution widths. The depth X=(1-20) nm covers the near-interface region, and Y=(0.5-3.5) μm covers the JFET, channel, and n+ source regions.
Vth, gm, and Ion were extracted as outputs. The reference values, excluding the effect of the traps, are Vth=2.894 V, gm=20.78 S, and Ion=45.86 A. The changes ΔVth, Δgm, and ΔIon are defined as the differences from these reference values under all conditions.

2.3. Device Degradation Characteristics Due to DDs

Figure 2 compares the ID-VGS curves for different lateral trap positions. At Y≥2.5 μm, the difference between Ion and the reference value is less than 0.2%, so all curves overlap with the reference curve. At Y=0.5 μm, the turn-on voltage remains unchanged, while the saturation current decreases to a minimum of 28 A. In contrast, at Y=1.0 μm and 1.5 μm, the entire curve shifts toward higher VGS values, and under some conditions, the device does not turn on at all even at VGS=10 V. The curve at Y=2.0 μm lies just below the reference curve, indicating relatively small degradation at this position.
Table 2 summarizes the maximum changes in Vth, gm, and Ion as all other variables were varied at each lateral position. At the JFET edge (Y=1.0 μm) and in the channel (Y=1.5 μm), Vth increased by up to 7.09 V, while both gm and Ion dropped to nearly zero. The JFET center (Y=0.5 μm) exhibited different behavior. While Vth remained unchanged, Ion decreased by up to 38%. Traps in the n+ source region beneath the gate (Y=2.0 μm) had a weaker effect, reducing gm and Ion by up to 31% and 11%, respectively. When the trap was outside the gate (Y≥2.5 μm), none of the three output parameters changed by more than 0.5%.
At the same Y, the difference in the maximum degradation with the depth X=(1-20) nm was small. This is because, in most conditions, σ is larger than the center depth, so the trap region extends to the interface. In contrast, under the condition of σ=10 nm and X=20 nm, where the trap region does not reach the interface, the maximum Ion reduction at Y=1.5 μm decreased from 100% at X≤15 nm to 17%. In addition, the degradation increased as the distribution width increased. The maximum Ion reduction at Y=0.5 μm was 9% for σ=10 nm and 38% for σ=100 nm, and at Y=1.0 μm it was 35% for σ=10 nm and 100% for σ=100 nm.
This positional selectivity is related to the charge state of the acceptor-like traps. In the JFET region, since the Fermi level is above the trap level, the traps capture electrons and become negatively charged, compensate for the donors, and deplete the accumulation path beneath the gate. In a planar MOSFET, electrons that have passed through the channel flow into the drift region via the accumulation layer on the surface of the JFET region. Therefore, when the negative charge of the traps reduces the electron concentration in the accumulation layer, the current is suppressed. In particular, the negative charge of the traps in the channel adds to the acceptors in the p-body, increasing the gate voltage required to form the inversion layer and thus directly raising Vth. At the JFET edge (Y=1.0 μm), the traps lie on the path through which electrons leaving the channel enter the JFET region; depleting this path keeps ID below Io up to a higher VGS, so the Vth extracted by the constant-current method increases even though the traps do not reach the channel.
Figure 3 shows Vth, gm, and Ion according to the trap concentration and energy level at Y=1.0 μm, X=8 nm, and σ=100 nm, among the most sensitive positions. Even at the lowest DD-induced trap concentration considered, 3×1016 cm-3, Ion decreased by 0.9-1.7%, and the degradation appeared continuously with concentration over the entire concentration range considered. At 3×1017-5×1017 cm-3 the Ion reduction was 2-10% and the Vth increase was within 1.8 V, and at 3×1018 cm-3, levels of 0.4 eV or deeper turned into severe degradation, with Ion decreasing by 37-100%. At this position, Vth increased by approximately 4 V at 0.8 eV and by approximately 7 V at 1.0 eV. The saturation concentration at which degradation ceased to increase was higher for shallower energy levels. Across the entire dataset, the concentration at which the maximum Ion reduction reached 100% was 3×1018 cm-3 at 0.8 eV or deeper, 5×1018 cm-3 at 0.6 eV, and 3×1019 cm-3 at (0.2–0.4) eV.
At the same concentration, ΔVth and ΔIon increase as the energy level becomes deeper. At Y=1.0 μm, shallow energy levels of 0.2 eV and 0.4 eV caused almost no change in Vth (less than 0.04 V), but Ion decreased to 6.9 A and 1.9 A, respectively, at 5×1019 cm-3. Shallow traps primarily capture electrons after turn-on, when the Fermi level approaches the conduction band; therefore, they affect Ion more than Vth. Deep traps carry a negative charge even before turn-on, causing Vth to shift. The energy level that distinguishes these two behaviors depends on the trap’s position. At 0.2 eV, Vth varied by no more than 0.1 V even at Y=1.0 and 1.5 μm. However, at Y=1.5 μm, levels of 0.4 eV and deeper caused Vth to rise by up to (3.3–7.1) V, whereas at Y=1.0 μm, this effect only occurred at levels of 0.6 eV and deeper.

3. Data Preprocessing and DNN Model Design

3.1. Data Preprocessing

Because radiation reliability assessment is the process of determining how much the device characteristics change under specific defect conditions, the conditions with large degradation are exactly the region where prediction is needed. However, in this region, the nonlinearity of the characteristics increases and the prediction error also increases; thus, removing such conditions from the training data would improve the metrics but would not secure the predictive capability that is actually needed. Therefore, only numerically invalid results were removed through preprocessing, and the application range was limited to the conditions that turn on within the gate sweep range.
A previous study compared the effect of data preprocessing on the prediction performance of DNNs in TCAD-based radiation degradation prediction [15]. Accordingly, Table 3 shows the content of each step and the numbers of removed and remaining data. Method I removed 436 conditions that did not converge and did not complete the calculation up to VGS=10 V. Method II covers 377 conditions in which the current decreased by 0.5 dec or more as the gate voltage increased after turn-on; a current decrease with increasing gate voltage cannot be explained physically and was therefore judged to be a numerical error and removed. Method III separated 86 conditions in which ID did not reach the reference current Io at VGS=10 V. For these conditions, Vth cannot be extracted within the sweep range, and gm and Ion are also not post-turn-on characteristics; therefore, to keep the same application range for the three models, these conditions were excluded from all three models. Method IV involves only scaling the input and output values without removing any data, and applies the standardization method used in a study on neural network-based prediction of SiC device characteristics [16]. Since the ranges and units of the input variables differed, to prevent variables with large magnitudes from dominating the learning process, the trap concentration Nt and the distribution width σ were converted to common logarithms and then z-score standardized so that each of the five inputs and output had zero mean and unit standard deviation. If the trap concentration were standardized using its original linear scale, six out of eight concentrations (3×1016–5×1018) cm-3 would be concentrated in a narrow range from −0.63 to −0.35, and the difference around 3×1017 cm-3 would be virtually indistinguishable in the input. Therefore, a log transformation was used to even out the concentration intervals. Since Ion is distributed over five orders of magnitude—from 10-3 to 4.6×101 A—even within the valid range, log10Ionwas used, and the predicted values were inverse-transformed after training. The mean and standard deviation used for standardization were calculated only from the training set, and the same values were applied to the validation and test sets.

3.2. DNN Configuration and Training

Since Vth, gm, and Ion are different physical quantities and exhibit different response patterns to concentration, they were trained using separate DNN models. All three models are fully connected neural networks that take five inputs and produce one output, and the hidden layers use the sigmoid linear unit (SiLU) activation function. We compared 16 combinations of hidden layer width (128, 256), depth (3, 4), learning rate (10-3, 5×10-4), and batch size (64, 128) based on validation loss. The selected architectures are shown in Table 4. The optimizer used was Adam, and the loss function was mean squared error (MSE). If the validation loss did not decrease for 40 epochs, the learning rate was halved. If it did not decrease for 120 epochs, training was terminated, and the weights with the minimum validation loss were adopted. The random seed used for data splitting, weight initialization, and mini-batch ordering was fixed at 42, and PyTorch was used for the implementation [17].
The dataset was partitioned into training, validation, and test sets at a ratio of 70:15:15. For all three models, the entire dataset of 10,301 conditions was split into 7,210/1,545/1,546 conditions, and the test set is common. The split was stratified by response (|ΔVth|≥0.01 V, |Δgm|≥0.1 S, or |ΔIon|≥0.1% of the reference Ion) so that the proportion of responsive samples is the same in the three subsets.
MAE = 1 N ∑ i = 1 N | y i − y i ^ |
R 2 = 1 − ∑ i = 1 N ( y i − y i ^ ) 2 ∑ i = 1 N ( y i − y ¯ ) 2
For the N samples in the test set, yi is the TCAD simulation value, y ^ i is the DNN prediction, and y ¯ is the mean of all yi in Equations (1) and (2). MAE is the mean of the absolute prediction errors and has the same unit as the output, so it directly shows how large the errors are. However, if most of the data is clustered around the reference value, even a model that simply outputs the reference value will yield a small MAE. R2 represents the proportion of the test set’s variance explained by the model. It is 0 if the model outputs only the mean and 1 if it predicts perfectly, thus indicating how well the model tracks variations in the data. Since the two metrics are complementary, they are presented together. For the Vth and gm models, the metrics were calculated after converting the predicted values on the standardized scale back to their original units (V, S). For the Ion model, whose values span five orders of magnitude within the valid dataset, the metrics were calculated in the log10Ion space. Since 57.6% of the test set did not meet the response criteria, the DNN’s performance metrics were calculated for both the entire test set and the 656 test samples that met the response criteria.

4. Prediction Results and Discussion

Figure 4 shows the parity plots of the three models trained with the architectures in Table 4 for the test set. Vth followed the diagonal over the entire range from the reference value of 2.89 V to 9.9 V near the turn-on limit; 42 conditions had errors exceeding 0.1 V, 14 conditions had errors exceeding 0.3 V, and the maximum error was 0.77 V. gm was reproduced from the (22-23) S region, which is larger than the reference value, down to the 10-3 S level; however, 17 conditions had errors exceeding 0.3 S, such as a condition of 0.69 S predicted as 8.9 S, and negative values as low as −0.18 S were predicted for some conditions with gm close to 0. This is because gm was trained on a linear scale; since gm≥0 physically, the predictions should be limited to 0 in application. Ion was predicted over five orders of magnitude from the reference value of 46 A to 1 mA; four conditions had log errors exceeding 0.3 dec, and the maximum error was 1.35 dec.
For the entire test set, the Vth model achieved R2=0.994 and MAE=0.011 V, the gm model achieved R2=0.997 and MAE=0.033 S, and the Ion model achieved R2=0.987 and MAE=0.0068 dec on the log scale. Even when evaluated only on the responsive samples, R2 was 0.994, 0.996, and 0.986 and MAE was 0.024 V, 0.072 S, and 0.015 dec, showing high prediction performance for the responsive samples as well.
Conditions with large errors mostly occurred in the severely degraded region where Y=(1.0–1.5) μm. Conditions with large Vth errors were primarily observed in the region where Y=1.0 μm, X=(10-20) nm, σ=(80-100) nm, and Nt≥5×1018 cm-3; this is the region where Vth rises sharply to (7-10) V. Large errors in gm and Ion were concentrated in the region where Y=1.5 μm, σ=(10-20) nm, and X=(10-15) nm. Under these conditions, the half-width of the trap is similar to the center depth, so whether the trap region touches the interface depends on small differences in X and σ, resulting in a sharp change in output. In other words, the errors in the DNN are concentrated at the boundary where the output changes sharply with respect to the input, while in other regions, the DNN quantitatively reproduces the changes in the three characteristics. Therefore, the degradation of 4H-SiC MOSFETs caused by DDs near the interface depends on the lateral position, energy level, concentration, and distribution width of the traps and on whether the trap region reaches the interface; within its valid range, the DNN can quantitatively predict degradation for various combinations of variables without TCAD simulation.

5. Conclusions

The DDs near the interface between the gate oxide and SiC in a 4H-SiC MOSFET were modeled as acceptor-like traps. TCAD simulations were performed using 11,200 conditions created by combining five parameters (energy level, concentration, depth, lateral position, and distribution width) and the resulting degradation of Vth, gm, and Ion was analyzed. When DDs were present near the interface, the factors influencing device degradation were their position, energy level, concentration, and whether they were in contact with the interface. First, the lateral position of the trap determined the degree of degradation, which was most severe in the channel (Y=1.5 μm) and at the JFET edge (Y=1.0 μm). At the center of the JFET (Y=0.5 μm), only Ion showed a reduction of up to 38% without any change in Vth, while there was almost no effect outside the gate. The degradation characteristics of the traps depending on their location can be explained by the fact that the negative charge of the electron-capturing traps hindered the formation of the inversion layer and the accumulation layer on the JFET surface. Shallow energy levels at 0.2 eV reduced Ion without shifting Vth, whereas levels at 0.4 eV and deeper increased Vth; these levels varied depending on the trap position. The effect became apparent starting at the lowest concentration of 3×1016 cm-3 even at (0.2-0.4) eV, with higher saturation concentrations observed at shallower energy levels. The depth from the interface itself had little effect; rather, it was critical whether the trap region touched the interface. When the trap region spanned the interface, the difference depending on the depth (1-20) nm was small, but degradation increased as the distribution width widened.
These factors interact, so degradation cannot be captured by a simple equation or by linear interpolation. A single TCAD run takes minutes to hours depending on the condition, and sweeping every combination of variables this way is not practical. We therefore preprocessed the 11,200 conditions, removing runs that did not converge, curves whose current fell non-physically after turn-on, and conditions in which the reference current was not reached within the sweep range. The DNN was trained on the remaining 10,301 valid conditions. On the test set it reached R²=0.994 (MAE=0.011 V) for Vth, R²=0.997 (MAE=0.033 S) for gm, and R²=0.987 (MAE=0.0068 dec) for log10Ion. Restricting the evaluation to the responsive samples, where the trap effect actually appeared, changed little: R² of 0.994, 0.996, and 0.986 with MAE of 0.024 V, 0.072 S, and 0.015 dec. The largest errors sit at boundaries where the output jumps with a small change in input; elsewhere the DNN reproduces the three characteristics quantitatively. The trained DNN thus predicts degradation for any near-interface trap condition within the valid dataset range without a TCAD run, and such predictions can be used to set design margins and test conditions for SiC power devices intended for radiation environments.

Author Contributions

Conceptualization, methodology, formal analysis, and writing—original draft preparation, G.P.; supervision and writing—review and editing, J.K. All authors have read and agreed to the published version of the manuscript.

Funding

This research was funded by by the Korea Institute of Energy Technology Evaluation and Planning (KETEP) and the Ministry of Climate, Energy & Environment (MCEE) of the Republic of Korea (No. RS-2026-25538218) and by by the KERI Primary research program of MSIT/NST (No. 26A01091).

Data Availability Statement

The data presented in this study are available on request from the corresponding author.

Acknowledgments

During the preparation of this manuscript, the authors used Claude (Opus 5.5, Anthropic) for the purposes of assisting with translation. The authors have reviewed and edited the output and take full responsibility for the content of this publication.

Conflicts of Interest

The authors declare no conflicts of interest.

Abbreviations

The following abbreviations are used in this manuscript:
DDs Displacement defects
DNN Deep neural network
JFET Junction field-effect transistor
MAE Mean absolute error
MOSFET Metal-oxide-semiconductor field-effect transistor
MSE Mean squared error
SiLU Sigmoid linear unit
TCAD Technology computer-aided design

References

  1. Kimoto, T.; Cooper, J.A. Fundamentals of Silicon Carbide Technology: Growth, Characterization, Devices and Applications; Wiley-IEEE Press: Singapore, 2014. [Google Scholar] [CrossRef]
  2. She, X.; Huang, A.Q.; Lucía, Ó.; Ozpineci, B. Review of Silicon Carbide Power Devices and Their Applications  . IEEE Trans. Ind. Electron. 2017, 64, 8193–8205. [Google Scholar] [CrossRef]
  3. Lauenstein, J.-M.; Casey, M.C.; Ladbury, R.L.; Kim, H.S.; Phan, A.M.; Topper, A.D. Space Radiation Effects on SiC Power Device Reliability  . In Proceedings of the 2021 IEEE International Reliability Physics Symposium (IRPS), Monterey, CA, USA, 21–25 March 2021; pp. 1–8. [Google Scholar] [CrossRef]
  4. Akturk, A.; McGarrity, J.M.; Wilkins, R.; Markowski, A.; Cusack, B. Space and Terrestrial Radiation Response of Silicon Carbide Power MOSFETs  . In Proceedings of the 2017 IEEE Radiation Effects Data Workshop (REDW), New Orleans, LA, USA, 17–21 July 2017; pp. 1–5. [Google Scholar] [CrossRef]
  5. Srour, J.R.; Marshall, C.J.; Marshall, P.W. Review of Displacement Damage Effects in Silicon Devices  . IEEE Trans. Nucl. Sci. 2003, 50, 653–670. [Google Scholar] [CrossRef]
  6. Hazdra, P.; Popelka, S. Radiation Resistance of Wide-Bandgap Semiconductor Power Transistors  . Phys. Status Solidi A 2017, 214, 1600447. [Google Scholar] [CrossRef]
  7. Hazdra, P.; Popelka, S. Displacement Damage and Total Ionisation Dose Effects on 4H-SiC Power Devices  . IET Power Electron. 2019, 12, 3910–3918. [Google Scholar] [CrossRef]
  8. Lee, G.; Ha, J.; Kim, K.; Bae, H.; Kim, C.-E.; Kim, J. Influence of Radiation-Induced Displacement Defect in 1.2 kV SiC Metal-Oxide-Semiconductor Field-Effect Transistors. Micromachines 2022, 13, 901. [Google Scholar] [CrossRef]
  9. Lee, G.; Kim, J. Effect of Radiation Displacement Defect on Superjunction MOSFET Using TCAD Simulation  . J. Inst. Electron. Inf. Eng. 2021, 58, 49–55. (In Korean) [Google Scholar] [CrossRef]
  10. Kim, J.; Kim, S.J.; Han, J.-W.; Meyyappan, M. Machine Learning Approach for Prediction of Point Defect Effect in FinFET  . IEEE Trans. Device Mater. Reliab. 2021, 21, 252–257. [Google Scholar] [CrossRef]
  11. Mehta, K.; Wong, H.-Y. Prediction of FinFET Current-Voltage and Capacitance-Voltage Curves Using Machine Learning with Autoencoder  . IEEE Electron Device Lett. 2021, 42, 136–139. [Google Scholar] [CrossRef]
  12. Synopsys. Sentaurus Device User Guide, Version R-2020.09; Synopsys, Inc.: Mountain View, CA, USA, 2020. [Google Scholar]
  13. Blakemore, J.S. Approximations for Fermi-Dirac Integrals, Especially the Function F_1/2 (η) UUsed to Describe Electron Density in a Semiconductor. Solid-State Electron. 1982, 25, 1067–1076. [CrossRef]
  14. Hatakeyama, T.; Fukuda, K.; Okumura, H. Physical Models for SiC and Their Application to Device Simulations of SiC Insulated-Gate Bipolar Transistors  . IEEE Trans. Electron Devices 2013, 60, 613–621. [Google Scholar] [CrossRef]
  15. Ryu, M.; Ha, J.; Lee, G.; Suh, M.; Bang, M.; Lee, D.; Kim, J. Prediction of Degradation Characteristics in Saddle Fin DRAM Due to Total Ionizing Dose and Displacement Defect Using Deep Neural Network  . J. Inst. Electron. Inf. Eng. 2023, 60, 29–37. (In Korean) [Google Scholar] [CrossRef]
  16. Niu, X.; Sang, L.; Duan, X.; Gu, S.; Zhao, P.; Zhu, T.; Xu, K.; He, Y.; Li, Z.; Zhang, J.; Jin, R. SiC MOSFET with Integrated SBD Device Performance Prediction Method Based on Neural Network  . Micromachines 2025, 16, 55. [Google Scholar] [CrossRef]
  17. Paszke, A.; Gross, S.; Massa, F.; Lerer, A.; Bradbury, J.; Chanan, G.; Killeen, T.; Lin, Z.; Gimelshein, N.; Antiga, L.; et al. PyTorch: An Imperative Style, High-Performance Deep Learning Library  . In Proceedings of the 33rd Conference on Neural Information Processing Systems (NeurIPS 2019), Vancouver, BC, Canada, 8–14 December 2019; pp. 8024–8035. [Google Scholar]
Figure 1. Structure and doping distribution of the simulated 4H-SiC MOSFET half-cell: (a) overall cross-section and (b) enlarged view of the gate region.
Figure 1. Structure and doping distribution of the simulated 4H-SiC MOSFET half-cell: (a) overall cross-section and (b) enlarged view of the gate region.
Preprints 238824 g001
Figure 2. Transfer characteristics (ID-VGS) for different lateral trap positions (Y). The dashed line indicates the reference curve.
Figure 2. Transfer characteristics (ID-VGS) for different lateral trap positions (Y). The dashed line indicates the reference curve.
Preprints 238824 g002
Figure 3. (a) Vth, (b) gm and (c) Ion as a function of trap concentration Nt for different trap energy levels Ec-Et at Y=1.0 μm, X=8 nm, and σ=100 nm. Dashed lines indicate the reference values, and the dotted line in (c) indicates the reference current Io=1 mA.
Figure 3. (a) Vth, (b) gm and (c) Ion as a function of trap concentration Nt for different trap energy levels Ec-Et at Y=1.0 μm, X=8 nm, and σ=100 nm. Dashed lines indicate the reference values, and the dotted line in (c) indicates the reference current Io=1 mA.
Preprints 238824 g003
Figure 4. Parity plots of the Vth, gm, and Ion models for (a-c) the whole test set (n=1546) and (d-f) the responsive samples only (n=656). R2 and mean absolute error (MAE) are given in each panel.
Figure 4. Parity plots of the Vth, gm, and Ion models for (a-c) the whole test set (n=1546) and (d-f) the responsive samples only (n=656). R2 and mean absolute error (MAE) are given in each panel.
Preprints 238824 g004
Table 1. Sweep variables of the technology computer-aided design (TCAD) simulation dataset.
Table 1. Sweep variables of the technology computer-aided design (TCAD) simulation dataset.
Variables Levels #
Energy level Ec-Et (eV) 0.2, 0.4, 0.6, 0.8, 1.0 5
Concentration Nt (cm-3) 3×1016, 5×1016, 3×1017, 5×1017,
3×1018, 5×1018, 3×1019, 5×1019
8
Depth X (nm) 1, 2, 4, 6, 8, 10, 15, 20 8
Lateral position Y (μm) 0.5, 1.0, 1.5, 2.0, 2.5, 3.0, 3.5 7
Trap half-width σ (nm) 10, 20, 50, 80, 100 5
Table 2. Maximum degradation relative to the reference values at each lateral trap position Y, evaluated over all turned-on conditions.
Table 2. Maximum degradation relative to the reference values at each lateral trap position Y, evaluated over all turned-on conditions.
Lateral position Y (μm) Max ΔVth
(V)
Max gm reduction
(%)
Max Ion reduction
(%)
0.5 (JFET center) 0.00 21 38
1.0 (JFET edge) 7.09 100 100
1.5 (channel) 7.08 100 100
2.0 (n+ source) 0.00 31 11
2.5 (n+ source) 0.00 0.2 0.1
3.0 (n+ source) 0.00 0.2 0.1
3.5 (n+ source) 0.00 0.5 0.1
Table 3. Data preprocessing steps.
Table 3. Data preprocessing steps.
Method Description Removed Remaining
I Removal of non-converged runs 436 10,764
II Removal of curves whose current decreases by more than 0.5 dec after turn-on 377 10,387
III Separation of runs without turn-on within the gate sweep (ID<Io at VGS=10 V) 86 10,301
IV log10(Nt), log10(σ) + z-score 0 10,301
Table 4. Selected deep neural network (DNN) architecture and hyperparameters.
Table 4. Selected deep neural network (DNN) architecture and hyperparameters.
Item Vth model gm model Ion model
Output Vth gm log10Ion
Hidden layer 128×4 256×4 128×4
Learning rate / batch size 5×10-4 / 128 5×10-4 / 64 5×10-4 / 128
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content.
Copyright: This open access article is published under a Creative Commons CC BY 4.0 license, which permit the free download, distribution, and reuse, provided that the author and preprint are cited in any reuse.