The microstructure and properties of diffusion aluminide coatings are strongly influ-enced by processing conditions, making their optimization essential for controlling coating development. This study investigated the effects of slurry aluminizing temper-ature and treatment time on coatings produced on X3CrTi17 ferritic stainless steel using an inorganic sodium silicate binder. Coatings were manufactured at 700, 800, and 1000 °C for 1, 2, and 6 h and characterized by microscopy, EDS, XRD, and nanoindentation. At 700–800 °C, coatings exhibited distinct compositional boundaries, with Al₅Fe₂ identified as the predominant near-surface phase. At 1000 °C, substantially thicker coatings de-veloped, characterized by an extended diffusion zone, gradual elemental gradients, and AlFe in the near-surface region. EDS analysis also revealed localized Si- and Cr-enriched regions. Empirical regression models described the dependence of coating thickness (R² = 0.981) and mass gain (R² = 0.978) on processing parameters. Nanoindentation revealed coating hardness of approximately 11 GPa, compared with 4–5 GPa for the substrate. The results demonstrate that processing temperature plays a key role in controlling phase formation, diffusion-zone development, and local mechanical properties of slurry alu-minide coatings.
Keywords:
slurry method
; aluminide coatings
; ferritic stainless steel
1. Introduction
Ferritic stainless steels are widely used in power-generation, solid oxide fuel cell (SOFC), and steam-turbine environments because of their cost and corrosion resistance, but their oxidation resistance can deteriorate above about 600°C, especially under cyclic or water-vapor exposure [1,2,3]. Aluminide coatings address this by promoting the formation of a dense, adherent Al2O3 scale that acts as a diffusion barrier and slows cation outward diffusion and substrate attack [4,5,6,7,8,9] . This topic matters because coated ferritic steels can offer a lower-cost alternative to more expensive alloy families while still extending service temperature and lifetime [10].
Across multiple studies, aluminide coatings substantially improved oxidation resistance of ferritic steels in air, steam, and water-vapor atmospheres[1,11,12,13,14,15]. In several cases, coated steels formed protective alumina scales that limited mass gain or reduced oxidation rates by orders of magnitude relative to uncoated substrates [13,16,17,18]. Long-duration exposure studies are especially strong: slurry aluminide coatings on ferritic steels remained very resistant in steam for 45,000–50,000 h in some reports, and CVD aluminide coatings on ferritic or stainless steels showed no failure after 10,000–16,000 h in humid atmospheres in another study [17,18,19].
The coating phase structure commonly evolves toward Al5Fe2, AlFe, or multilayer Fe-Al intermetallic architectures depending on process temperature and time [11,20,21,22]. That microstructure matters because protective behaviour is linked to the ability to sustain a continuous alumina film; when voids, cavities, or cracks form at the coating/oxide or coating/substrate interface, spallation risk increases [1,23,24]. Several studies explicitly report Kirkendall porosity, interface voids, or cracking as the main durability limit, not the absence of initial coating formation [17,23,25,26,27].
Low-temperature aluminizing can preserve substrate properties but often favours inward growth and brittle η-Al5Fe2-type structures; higher-temperature treatments can improve phase stability and surface quality, yet increase diffusion and grain growth in the substrate [5,21,23,28]. This creates a practical design window: many papers target roughly 650–700°C for service or deposition-related treatments, while some CVD/pack routes use 800–1050°C to tailor phase constitution and coating stability [1,11,13,28,29].
Reactive additions such as Zr, Ce, La, Y2O3, Hf, or Cr enrichment are repeatedly associated with improved alumina adhesion, reduced cracking/spallation, or faster stabilization of α-Al2O3 [14,15,24,28,30,31,32]. However, the benefit is composition- and dosage-dependent: excess CeCl3 worsened oxidation in one study by increasing porosity, so additive optimization is essential.
The performance of aluminide coatings on ferritic stainless steels depends not only on their aluminium content but also on the manufacturing method, phase evolution, and stability of the coating–substrate interface [12,13,17,23,24,25,28]. Among the available techniques, slurry aluminizing is particularly attractive for steam-service applications, while CVD/CVD-FBR enables controlled coating chemistry and pack cementation offers a cost-effective diffusion treatment for complex geometries [5,6,11,20,33]. Nevertheless, long-term exposure and thermal cycling may lead to diffusion-driven degradation, cracking, Kirkendall porosity, and oxide-scale spallation [1,23,24,25,28,34]. Previous studies have demonstrated the potential of slurry aluminide coatings to provide long-term oxidation resistance on ferritic steels, although coating integrity and microstructural stability remain important challenges [11,12,25,26].
Although aluminide coatings on ferritic stainless steels have been extensively investigated, understanding the relationships between processing parameters, coating growth, phase evolution, and local mechanical properties remains important for controlling their microstructure. In particular, changes in processing temperature and treatment time may simultaneously affect the formation of Fe–Al intermetallic compounds, the development of diffusion zones, and the redistribution of alloying elements such as Cr and Si. These processes can produce chemically and structurally heterogeneous coatings with different local mechanical responses. Therefore, a combined analysis of coating thickness, elemental distribution, phase composition, and mechanical properties is necessary to better understand the evolution of aluminide coatings under different processing conditions.
In this work, diffusion aluminide coatings were produced on X3CrTi17 ferritic stainless steel using the slurry cementation method with an inorganic binder. Compared with conventional chemical vapour deposition and halide-activated pack cementation, the slurry method offers flexibility in coating application, allowing components of different shapes and dimensions, as well as selected surface areas, to be treated. An important feature of the applied approach is the use of sodium silicate (water glass) as an inorganic binder, which provides sufficient cohesion of the dried slurry during specimen handling and subsequent heat treatment, without requiring a separate binder-removal stage.
The aim of this study was to investigate the influence of aluminizing temperature and treatment time on the microstructure, chemical and phase composition, growth behaviour, and local mechanical properties of diffusion coatings formed on X3CrTi17 ferritic stainless steel. Particular attention was paid to the formation of individual coating sublayers, the development of the coating–substrate transition region, and the relationship between chemical heterogeneity and mechanical response.
The study combines microstructural observations, EDS elemental analysis and spectral classification, X-ray diffraction, nanoindentation, and quantitative analysis of coating growth. This approach enables the temperature-dependent evolution of the coatings to be examined from both structural and mechanical perspectives. In addition, an empirical regression model was developed to describe the relationship between total coating thickness and processing parameters within the investigated experimental range.
2. Materials and Methods
2.1. Samples
The material used in this study was ferritic stainless steel X3CrTi17 (1.4510), with the nominal chemical composition specified in EN 10088-1 (wt.%): C ≤ 0.05, Si ≤ 1.00, Mn ≤ 1.00, P ≤ 0.040, S ≤ 0.015, Cr = 16.0–18.0, and Ti = 4(C + N) + 0.15 to 0.80. The balance was Fe. The specimens were cut from a cylindrical rod with a diameter of 25 mm into 4 mm thick discs. Each disc was then cut in half along its diameter. The samples were mechanically grounded and cleaned in an acetone bath before being immersed in the slurry. The composition of the slurry was established experimentally. The basic ingredients of the slurry were: an inorganic binder (an aqueous solution of sodium silicate) and a flux (a mixture of fused sodium and potassium salts: NaF, NaCl and KCl). The proportions of aluminium and silicon powders in the slurry were 9:1. The proportions of the first two components of the slurry, i.e. the sodium silicate and molten salts, refer to the sum of the weight of Al and Si powders. The ratio of the sodium silicate to powders of aluminium and silicon and the ratio of the salts to powders was 15/100 and 9.5/100, respectively. The powder size used was approximately 100 μm for aluminium and within the range 200–250 μm for silicon.
Figure 1.
Shape of the specimens used in this study.

The samples were immersed in the slurry and subsequently dried. The immersing and drying operations were repeated several times where necessary until the slurry mass value achieved the appropriate amount: 0.1 g/cm2.
The samples, covered with the slurry, were annealed in an argon atmosphere at 700, 800 and 1000 °C for 1, 2 and 6 hours (Table 1). The experimental design was initially based on a two-factor, two-level factorial design (2²), with annealing temperatures of 800 and 1000 °C and treatment times of 2 and 6 h. The experimental matrix was subsequently expanded to include a lower temperature of 700 °C, representing the minimum processing temperature considered for this method, and a shorter treatment time of 1 h. These additional conditions were introduced to investigate whether comparable coatings could be obtained under less demanding processing conditions, particularly in comparison with those produced at 800 °C for 2 h. After annealing, the slurry residues were mechanically re-moved, and the samples were washed in an ultrasonic bath in acetone. The residues easily detached from the surface after annealing.
Following annealing at the selected temperatures, diffusion coatings were formed, and the mass gain per unit surface area varied depending on the process parameters, as shown in Figure 2. Values are presented as mean ± standard deviation (SD), based on two independently prepared specimens (n = 2).
2.2. Microstructural Characterization
The specimens were mounted in a conductive resin (Polyfast, Struers, Ballerup Denmark) and subjected to mechanical grinding and polishing using a 0.25 µm diamond suspension. No polishing using a silica or alumina suspension was applied. The sample preparation procedure culminated with the implementation of low-angle (7°) argon ion milling using the Flat Milling System IM-3000 (Hitachi, Naka, Japan). The microstructure of the coatings was examined on cross-sections using field emission scanning electron microscopy (FE-SEM) – Hitachi SU-70 (Hitachi, Naka, Japan) with X-ray microanalysis energy dispersive spectrometry (EDS) – Thermo Scientific NORAN System 7 (Madison, WI USA), acceleration voltage 15 kV. The COMPASS software was used by collecting a complete, deadtime-corrected spectrum at every point of the sample. COMPASS is a statistical based software applied in the Thermo Noran 7 software which enables quantitative analysis of each elemental phase. The COMPASS software finds image locations that have the same spectral “fingerprint”, with no assumptions about the chemical composition of the sample. Such created elemental phase maps show the spatial distribution of regions that have statistically similar spectral features (peak locations and relative peak heights) and cumulative spectra of these regions.
X-ray diffraction (XRD) phase analysis was performed using Cu-Kα, using X-ray tube parameters of 35 kV and 45 mA and a Bragg–Brentano geometry (X’Pert–PRO, Panalytical, Almelo, The Netherlands). The applied step of the goniometer was 0.05°, and the acquisition time was 200 s. The acquired data were processed using X’Pert HighScore (v. 2.2.1) software provided by Panalytical.
Hardness and reduced elastic modulus were determined by nanoindentation using a Hysitron TI 950 nanoindenter (Bruker Corporation) equipped with a Berkovich diamond indenter. Measurements were performed on polished cross-sections using the Accelerated Property Mapping (XPM) technique to acquire spatial distribution of indentation hardness and reduced elastic modulus [35]. Each map consisted of an array of individual indents applied using an identical trapezoidal load function under load-controlled feedback: loading to a peak force of 1 mN over 0.1 s, holding at peak load for 0.1 s, and unloading over 0.1 s. The lateral spacing between adjacent indents was set to 1 µm. For all measurements, the maximum contact depth remained below 100 nm. The acquired load-displacement data were processed and analyzed using Origin 2021 (OriginLab Corporation) in combination with the XPM Mapping and Statistics add-on (Bruker Corporation).
3. Results
3.1. Microstructure of Coatings
Coatings were manufactured under an argon atmosphere using the parameters listed in Table 1. Each coating consisted of several identifiable sub-layers. The sub-layers were numbered sequentially starting from the substrate. Representative micrographs illustrating the microstructures of all coatings produced under different processing conditions are presented in Figure 3. Due to variations in coating thickness, different magnifications were used in the images to present as many microstructural details as possible.
The thickness of the coatings depending on the manufacturing parameters used is shown in Figure 4. The thicknesses of individual coating sublayers were determined from optical and scanning electron microscopy images of cross-sectional specimens. Multiple measurements were performed at different locations within each specimen. At each measurement location, the thicknesses of all identified sublayers were measured, and their sum was used to calculate the total coating thickness. The results are expressed as mean values and standard deviations (SD), reflecting the local thickness variations within each coating. One specimen was examined for each combination of processing temperature and treatment time.
A regression model describing the relationship between the total coating thickness and the processing parameters was developed using the multiple regression module in Statistica 13.0 software:
YT = 1482,170-3,638·X1+ 0,002272778·X12-51,557·X2-4,826·X22+0,118·X1·X2,
The following notation was used: YT – the thickness of the coatings (µm); X1 – the annealing temperature (°C); X2 – the annealing time (h). The graphical representation of the model is presented in Figure 5a. Additionally, regression analysis was performed to investigate the relationship between mass change (Figure 2) after the aluminizing process and the processing parameters:
YM = 0,011720-0,007957·X2+0,000012·X1·X2,
The following notation was used: YM – the mass changes (g/cm2); X1 – the annealing temperature (°C); X2 – the annealing time (h). The graphical representation of the model is presented in Figure 5b.
The second-order polynomial regression model (1) provided a good description of the relationship between coating thickness, processing temperature, and treatment time within the investigated experimental range (R² = 0.981, adjusted R² = 0.949). The nonlinear character of this relationship is consistent with the temperature-dependent evolution of the coating microstructure and phase composition. In particular, the transition from Al₅Fe₂-rich near-surface regions at 700–800 °C to AlFe-rich regions at 1000 °C, accompanied by the development of an extended diffusion zone, suggests that coating growth is governed by a combination of thermally activated diffusion and phase formation processes. Therefore, the regression equation should be regarded as an empirical description of the experimental results rather than a universal kinetic model. Its applicability is restricted to the investigated temperature range of 700–1000 °C and treatment times of 1–6 h, and extrapolation beyond these conditions is not justified without additional experimental verification.
A similar relationship was observed for the mass change per unit surface area after the aluminizing process (Figure 5b). The regression model (2) also exhibited a very good fit to the experimental data (R = 0.989, R² = 0.978, adjusted R² = 0.971, F(2,6) = 134.27, p < 0.00001). The positive temperature–time interaction term indicates that the influence of treatment time on mass gain becomes more pronounced at higher processing temperatures. This trend is consistent with the coating thickness results, suggesting that both mass gain and coating growth are strongly influenced by the combined effects of temperature and treatment time. The agreement between these two experimentally determined parameters supports the interpretation of enhanced diffusion and aluminide layer development at elevated temperatures.
3.2. EDS Chemical Composition
The EDS elemental maps presented in Figure 6 illustrate the distribution of Al, Si, Ti, Cr, and Fe within the aluminide coatings produced at different temperatures for a constant treatment time of 1 h. The results reveal chemically distinct regions characterized by variations in elemental concentrations. The outer coating regions exhibit a high Al content, whereas Fe concentration increases towards the substrate. Chromium is detected throughout the coating and substrate, while silicon exhibits local variations in its distribution. Increasing the treatment temperature from 700 to 1000 °C is accompanied by changes in the elemental distribution and the development of a more extended diffusion zone.
The EDS line scans and point analyses presented in Figure 7 and Table 2 provide further insight into the chemical composition of the aluminide coating produced at different temperatures for a constant treatment time of 2 h. At 700 °C, the outer region is characterized by a high Al content of 72.3 at.% and an Fe content of 26.3 at.% (point 1). A similar composition was observed at 800 °C, with Al and Fe concentrations of 68.6 and 30.5 at.%, respectively (point 4). These compositions are consistent with the stoichiometry of the Al5Fe2, intermetallic phase, suggesting its possible formation the Al-rich regions of the coatings. Furthermore, according to the Al-Fe-Cr-Si phase diagram [36], the presence of Cr and Si may favour the stability of Al5Fe2 over more Al-rich phases, such as Al13Fe4.
Further EDS analysis revealed local variations in the Al-to-Fe atomic ratio within the coatings. At 800 °C, an area containing 47.7 at.% Al and 45.5 at.% Fe was identified (point 7), while a comparable composition was observed at 1000 °C, with 44.6 at.% Al and 48.2 at.% Fe (point 9). These compositions are close to the equiatomic Al-to-Fe ratio, suggesting the possible presence of AlFe-type intermetallic regions. The presence of chromium in these regions indicates that the intermetallic phase may also accommodate a certain amount of Cr in its structure.
An additional feature was observed in the coating produced at 800 °C (point 6), where relatively high concentrations of chromium and silicon were detected. When the Al and Fe contributions are excluded, the atomic ratio of Cr to Si approaches the stoichiometry of Cr₃Si. This suggests that the corresponding precipitates may represent chromium silicide. However, the measured Al and Fe contents may partly originate from the surrounding matrix due to the limited spatial resolution of EDS analysis. Therefore, the assignment of these precipitates to Cr₃Si should be regarded as a probable interpretation based on their chemical composition and previous observations of this phase in comparable materials.
The EDS line profiles and corresponding BEI micrographs (Figure 7) reveal distinct differences in elemental distribution and coating morphology depending on the treatment temperature. At 700 and 800 °C (Figure 7a,b), a relatively sharp decrease in the Al signal intensity, accompanied by an increase in the Fe signal intensity, is observed at the coating–substrate interface. These compositional changes are consistent with a reactive diffusion mechanism, leading to the formation of chemically distinct regions separated by relatively well-defined interfaces. The local chemical composition at the transition between the coating and the substrate may also indicate the presence of Al-enriched Fe–Cr regions, potentially corresponding to a solid solution formed through the incorporation of aluminium into the ferritic matrix. However, the available EDS data do not allow an unambiguous distinction between such a solid solution and Fe-rich aluminide regions containing chromium.
In contrast, the coating produced at 1000 °C (Figure 7c) exhibits a gradual decrease in the Al signal intensity and a corresponding increase in the Fe signal intensity over a considerably greater distance, without a clearly defined reaction front. This behaviour suggests enhanced interdiffusion at elevated temperatures, resulting in the development of an extended diffusion zone characterized by a gradual change in chemical composition. The point analyses performed across this region further support this interpretation. In particular, the local Al concentration decreases from 44.6 at.% in the outer region (point 9), through 25.1 at.% (point 10), to 15.2 at.% closer to the substrate (point 11). Simultaneously, the Fe and Cr contents increase, indicating a gradual transition towards the composition of the underlying ferritic steel.
The composition of the intermediate region, particularly at point 10, is also noteworthy, as its Al content is close to the nominal stoichiometry of Fe₃Al. This may suggest the presence of an Al-rich Fe–Cr region with a composition derived from Fe–Al intermetallic phases. However, considering the significant chromium content and the absence of crystallographic information for individual regions, the formation of a specific ordered phase, such as Fe₃Al, cannot be confirmed. Alternatively, these regions may represent an aluminium-containing Fe–Cr solid solution, potentially involving different degrees of atomic ordering. Such a compositional transition may reflect the progressive development of a diffusion zone between the Al-rich intermetallic coating and the ferritic substrate, rather than the formation of several discrete intermetallic layers. It should also be considered that the structural state of these regions may change during cooling from the processing temperature.
To further examine the chemical heterogeneity of the coatings, EDS spectral classification using the COMPASS method was performed for representative samples produced at 700 and 1000 °C. The resulting maps, presented in Figure 8, distinguish regions with different characteristic EDS spectra, while their average chemical compositions are summarized in Table 3.
For the coating produced at 700 °C, five chemically distinct regions were distinguished. The main coating region (Phase 1) contained 66.0 at.% Al and 28.7 at.% Fe, suggesting the presence of an Al₅Fe₂-type intermetallic phase. The region corresponding to the substrate (Phase 2) was predominantly composed of Fe and Cr. In addition, a narrow Si-enriched region (Phase 3), containing 21.4 at.% Si, was identified within the coating. Dispersed precipitates enriched in Cr and Si (Phase 4) were also observed. Their Cr-to-Si atomic ratio was close to 3:1 when considering only these two elements, suggesting the possible presence of Cr₃Si. Another Al-rich region (Phase 5), containing 10.4 at.% Si, was predominantly located in the outer part of the coating.
In contrast, three chemically distinct regions were identified in the sample produced at 1000 °C. The outer coating region (Phase 7) contained 37.9 at.% Al and 53.3 at.% Fe, suggesting the possible presence of an Fe-rich AlFe-type intermetallic phase. Towards the substrate, an extended region (Phase 6) containing 10.4 at.% Al, 76.2 at.% Fe and 11.8 at.% Cr was distinguished. Its composition is consistent with an Al-enriched Fe–Cr solid solution. Additionally, dispersed Cr-rich precipitates (Phase 8), containing 49.6 at.% Cr and 45.5 at.% Fe, were observed mainly in the inner region of the coating and near the substrate. Their low Si content does not support their identification as chromium silicides. Their chemical composition and spatial distribution suggest the possible presence of chromium-rich precipitates, potentially carbides of the M₂₃C₆ type. However, their precise identification was not possible because carbon was not quantified in the EDS analysis.
The COMPASS analysis complements the EDS point and line measurements by revealing the spatial distribution of chemically distinct regions. The results demonstrate differences in elemental partitioning between coatings produced at 700 and 1000 °C, including the occurrence of Si-enriched regions at the lower temperature and an extended Al-containing Fe–Cr region at the higher temperature. Nevertheless, the spectral classes identified by COMPASS represent regions with similar chemical signatures and do not necessarily correspond to individual crystallographic phases.
Overall, the EDS results indicate that the chemical composition of the aluminide coatings varies with treatment temperature and distance from the surface. The observed differences in the Al-to-Fe atomic ratio suggest the presence of chemically distinct regions, potentially corresponding to different intermetallic compounds or aluminium-containing solid solutions. While coatings produced at 700 and 800 °C exhibit relatively distinct compositional boundaries, the coating formed at 1000 °C is characterized by an extended diffusion zone with a continuous chemical gradient towards the substrate. Their identification requires complementary crystallographic analysis, which is presented in Section 3.3.
3.3. Phase Analysis
X-ray diffraction (XRD) analysis was performed to identify the crystalline phases present in the near-surface regions of the aluminide coatings and to complement the EDS results. Figure 9 presents the XRD patterns of the untreated steel substrate and the coatings produced at different temperatures and treatment times.
The diffraction peaks of the substrate correspond to alloyed ferrite, whereas the coatings produced at 700 and 800 °C exhibit characteristic reflections of the Al₅Fe₂ intermetallic phase, regardless of treatment time. In contrast, the coatings produced at 1000 °C are characterized by diffraction peaks assigned to the AlFe intermetallic phase. These results indicate that the phase composition of the near-surface regions is primarily influenced by treatment temperature, with Al₅Fe₂ dominating at 700–800 °C and AlFe at 1000 °C. The identified phases are consistent with the local chemical compositions determined by EDS (Section 3.2). It should be emphasized that the XRD measurements were performed on the coating surfaces and therefore do not provide direct phase identification of the individual zones observed across the coating cross-sections. Consequently, the presence of additional intermetallic phases or solid solutions within the inner coating regions cannot be excluded.
3.4. Nanoindentation
The mechanical properties of the aluminide coatings were evaluated by nanoindentation to determine the distribution of hardness and reduced elastic modulus across the coating thickness. Figure 10 presents the corresponding BEI micrographs and mechanical property maps for selected coatings produced under different treatment conditions.
The analysed aluminide coatings exhibit hardness values of approximately 11 GPa, whereas the steel substrate is characterized by considerably lower values of approximately 4–5 GPa. The increased coating hardness is associated with the formation of Al–Fe intermetallic compounds identified by XRD analysis in Section 3.3. Although Al5Fe2 was the dominant phase in the coatings produced at 700 and 800 °C, while AlFe was identified at 1000 °C, the analysed coatings exhibited comparable general hardness levels. However, the measured values represent the local response of the multiphase coating microstructure and should not be interpreted as the intrinsic hardness of the individual intermetallic phases.
The reduced elastic modulus maps generally reveal lower values within the aluminide coatings than in the steel substrate, indicating differences in the local elastic response of these regions. The substrate exhibits values of approximately 200–220 GPa, consistent with the literature data reported for ferritic stainless steels. The spatial variations in reduced elastic modulus across the coating thickness are consistent with the changes in chemical composition and microstructure revealed by the EDS analysis in Section 3.2.
In the coatings produced at 700 and 800 °C, localized regions with increased hardness, typically ranging from 14 to 16 GPa and occasionally reaching approximately 19 GPa, were observed. Based on the corresponding elemental distributions, these regions may be associated with Cr- and Si-rich precipitates, potentially corresponding to Cr3Si precipitates [37], although their phase identification requires further crystallographic confirmation. In the coating produced at 1000 °C, localized regions with hardness values of approximately 16–17 GPa were also observed and may be associated with the Cr-rich features identified in the microstructure [38].
The mechanical property maps also demonstrate differences in the transition between the coating and the substrate. For the coating produced at 800 °C for 2 h, a relatively distinct transition between the harder aluminide coating and the softer steel substrate is visible. In contrast, the coating produced at 1000 °C for 6 h exhibits a more gradual variation in mechanical properties. This observation is consistent with the extended diffusion zone and continuous compositional gradient revealed by the EDS analysis.
4. Discussion
4.1. Effect of Processing Parameters on Coating Growth and Diffusion Behaviour
The growth of aluminide coatings on X3CrTi17 ferritic stainless steel was strongly influenced by the processing temperature and treatment time. However, the relative importance of these parameters varied considerably across the investigated temperature range. At 700 and 800 °C, the total coating thickness showed relatively limited changes with increasing treatment time, whereas at 1000 °C, a substantial increase in thickness was observed. This behaviour indicates that temperature plays a particularly important role in controlling the diffusion and reaction processes responsible for coating development. The extension of the experimental design to lower processing temperatures and shorter treatment times demonstrated that coatings with thicknesses comparable to those obtained at 800 °C for 2 h (approximately 93 µm) could also be produced at 700 °C for 2 h (approximately 84 µm) and 800 °C for 1 h (approximately 85 µm). In previous studies on slurry aluminizing, relatively long heat treatment times of 10 h or more have often been employed at temperatures around 700 °C [11,17]. In contrast, the present results demonstrate that coatings of considerable thickness can be obtained after only 2 h at 700 °C. These findings suggest that reducing either the processing temperature or treatment time may be feasible without a substantial reduction in coating thickness. However, similar thicknesses do not necessarily imply equivalent microstructures or functional properties, which should also be considered when selecting the optimal processing conditions.
The temperature dependence of coating growth can be related to the thermally activated diffusion of aluminium and iron and the formation of successive reaction products. At lower temperatures, the development of intermetallic layers may be restricted by relatively slow atomic transport and the presence of phase boundaries acting as additional diffusion barriers. Increasing the temperature to 1000 °C enhances interdiffusion and promotes the development of a considerably thicker reaction zone extending towards the substrate.
The kinetic analysis provides further insight into the coating growth mechanism. At 1000 °C, the approximately linear relationship between coating thickness and the square root of treatment time is consistent with diffusion-controlled growth. As the coating thickness increases, the diffusion distance becomes greater, progressively reducing the growth rate. However, the deviations from parabolic behaviour observed at 700 and 800 °C suggest that the growth mechanism cannot be adequately described by a single kinetic relationship over the entire investigated temperature range. The formation of different intermetallic phases and the evolution of individual reaction zones may contribute to these differences.
The empirical regression model further confirmed the combined influence of temperature and treatment time on total coating thickness. The second-order polynomial model provided a high coefficient of determination (R² = 0.981), indicating a good fit to the experimental data. Nevertheless, the model should be considered a descriptive tool rather than a physical representation of diffusion kinetics. Its applicability is restricted to the investigated temperature range of 700–1000 °C and treatment times of 1–6 h. In particular, changes in phase constitution and diffusion mechanisms may limit its predictive capability outside these conditions.
An additional feature observed in the coating microstructures was the variation in the morphology of the coating–substrate interface (Figure 3). At 800 °C, particularly after 1 h of treatment, the interface exhibited a pronounced wavy, locally tongue-like morphology, while similar irregularities became apparent at 700 °C after prolonged annealing (6 h). Such morphology has been associated in previous studies with preferential growth of the Al₅Fe₂ phase along the crystallographic c-axis, facilitated by structural vacancies that provide rapid diffusion pathways. Silicon has been reported to suppress this preferential growth by hindering diffusion through these pathways [39,40,41,42]. Interestingly, EDS point analysis revealed 0.9 at.% Si in an Al₅Fe₂-type region of the coating produced at 700 °C for 2 h, whereas no Si was detected at the corresponding point in the coating produced at 800 °C for 2 h (Table 2). This interpretation is further supported by the EDS elemental maps (Figure 6), which show that, in the coating produced at 800 °C, silicon is mainly concentrated in localized Cr-rich regions rather than being uniformly distributed within the Al₅Fe₂-rich layer. This difference is qualitatively consistent with the more pronounced interface irregularities observed at 800 °C. However, the local EDS measurements do not establish the silicon distribution at the reaction front or confirm the proposed diffusion mechanism. At 1000 °C, the absence of a distinct wavy front may instead be associated with the development of an extended interdiffusion zone and the formation of Fe-richer aluminide phases.
4.2. Phase Evolution and Development of the Coating–Substrate Transition Region
The evolution of coating microstructure was accompanied by significant changes in phase constitution and elemental distribution. At 700 and 800 °C, XRD analysis identified Al₅Fe₂ as the predominant crystalline phase in the near-surface region [43]. This identification is consistent with the high aluminium concentrations determined by EDS. The formation of Al-rich intermetallic compounds is characteristic of reactive diffusion in the Fe–Al system, where differences in elemental mobility and local chemical composition influence the development of successive reaction products.
At 1000 °C, AlFe became the predominant phase identified by surface XRD. This change was accompanied by a considerable increase in coating thickness and the development of an extended diffusion zone. The transition from Al₅Fe₂-rich to AlFe-rich near-surface regions suggests that increasing the processing temperature promotes more extensive interdiffusion and the formation of Fe-richer aluminides. The presence of chromium and silicon may additionally influence the stability and composition of the resulting intermetallic phases.
An important feature of the coatings produced at 1000 °C is the gradual decrease in aluminium concentration towards the substrate, accompanied by increasing iron and chromium contents. Unlike the relatively distinct compositional boundaries observed at lower temperatures, this transition region exhibits a continuous chemical gradient. Such behaviour suggests that coating development involves not only the formation of discrete intermetallic layers but also the progressive enrichment of the ferritic substrate with aluminium.
The intermediate regions may therefore contain aluminium-bearing Fe–Cr solid solutions or Fe-rich aluminide phases with different degrees of atomic ordering. In particular, local compositions approaching the Fe₃Al stoichiometry suggest the possibility of ordered Fe–Al-based structures. However, EDS measurements alone cannot distinguish between disordered and ordered solid solutions or confirm the presence of individual crystallographic phases. Moreover, the structural state of these regions may change during cooling from the processing temperature.
It should also be emphasized that the XRD measurements were performed on coating surfaces and therefore primarily characterize the near-surface phase constitution. Consequently, the identification of AlFe at 1000 °C does not imply that the entire coating consists of this phase. The combined XRD and cross-sectional EDS results instead suggest the development of a chemically graded coating, extending from the intermetallic-rich outer region towards the aluminium-enriched ferritic substrate.
Such a gradual compositional transition may also influence the distribution of mechanical properties across the coating–substrate interface, potentially reducing abrupt differences between the coating and substrate. However, its influence on interfacial stresses, adhesion, or cracking resistance requires further investigation.
4.3. Redistribution of Alloying Elements and Formation of Secondary Phases
In addition to the formation of Fe–Al intermetallic compounds, the aluminizing process resulted in local redistribution of chromium and silicon. The EDS point analyses and COMPASS spectral classification revealed chemically distinct regions enriched in these elements, indicating that coating formation involves more complex reactions than interdiffusion between aluminium and iron alone.
In the coatings produced at lower temperatures, localized regions with elevated chromium and silicon concentrations were identified. Their chemical composition suggests the possible formation of chromium silicides, particularly Cr₃Si-type precipitates. However, the measured compositions also contain significant amounts of aluminium and iron, which may partly originate from the surrounding matrix due to the finite interaction volume of the electron beam. Therefore, the identification of these regions as chromium silicides remains tentative.
The COMPASS analysis additionally revealed a Si-enriched region within the coating produced at 700 °C, together with chemically distinct Al-rich regions containing different silicon concentrations. These observations suggest that silicon is not uniformly incorporated into the growing aluminide coating but may be locally enriched in selected reaction zones. Such elemental partitioning may influence the formation and stability of individual intermetallic phases.
At 1000 °C, a different distribution of alloying elements was observed. In particular, chromium-rich precipitates were identified within the inner coating region and near the substrate. Their relatively low silicon content does not support their interpretation as chromium silicides. Considering their chemical composition and spatial distribution, these precipitates may represent chromium-rich carbides, potentially of the M₂₃C₆ type. However, because carbon was not quantified in the present EDS analysis, their identification remains uncertain.
The occurrence of these chemically distinct regions indicates that the diffusion aluminizing process involves redistribution of alloying elements originally present in the steel substrate. Their formation may be influenced by local changes in chemical composition and phase stability during coating growth. Nevertheless, the COMPASS spectral classes should not be interpreted as direct crystallographic phase identification, since regions with similar EDS spectra do not necessarily represent single phases.
4.4. Relationship Between Coating Microstructure and Mechanical Properties
The mechanical properties of the aluminide coatings reflect their complex microstructure and chemical heterogeneity. Nanoindentation measurements revealed substantially higher hardness within the coatings than in the ferritic steel substrate, which can be associated with the formation of Fe–Al intermetallic compounds. Although different predominant near-surface phases were identified at 700–800 °C and 1000 °C, the coatings exhibited broadly comparable hardness levels, suggesting that the presence of hard aluminide regions plays an important role in their local mechanical response.
The spatial distribution of hardness was not uniform across the coating thickness. Local variations may be related to changes in chemical composition, phase constitution, and the presence of secondary precipitates. In particular, regions enriched in chromium and silicon exhibited increased hardness, consistent with the possible occurrence of hard chromium-containing compounds. However, assigning specific hardness values to individual phases requires caution because the nanoindentation response may be affected by neighbouring phases, local microstructural heterogeneity, and the indentation depth.
The reduced elastic modulus values obtained for the aluminide coatings were generally lower than those measured for the ferritic steel substrate. This observation demonstrates that increased hardness does not necessarily correspond to increased elastic stiffness. Consequently, both hardness and reduced elastic modulus should be considered when evaluating the local mechanical behaviour of the coatings.
The development of an extended diffusion zone at 1000 °C may additionally contribute to a more gradual transition in mechanical properties between the coating and substrate. This interpretation is consistent with the observed compositional gradients, although a direct relationship between the diffusion-zone structure and mechanical performance requires further experimental verification.
5. Conclusions
The influence of processing temperature and treatment time on the microstructure, phase composition, growth behaviour, and local mechanical properties of slurry aluminide coatings produced on X3CrTi17 ferritic stainless steel was investigated. Based on the experimental results, the following conclusions can be drawn:
- Processing temperature was the dominant factor affecting coating development. At 700 and 800 °C, coating thickness showed relatively limited changes with increasing treatment time, whereas at 1000 °C, a substantial increase in thickness was observed. The results indicate enhanced interdiffusion and more extensive development of the reaction zone at elevated temperatures.
- The phase composition of the near-surface coating regions depended strongly on processing temperature. XRD analysis identified Al₅Fe₂ as the predominant phase at 700–800 °C and AlFe at 1000 °C. The higher processing temperature also promoted the formation of an extended diffusion zone characterized by a gradual decrease in aluminium concentration towards the substrate, in contrast to the relatively distinct compositional boundaries observed at lower temperatures.
- EDS analysis revealed redistribution of alloying elements during coating formation. Localized Si- and Cr-enriched regions were identified in coatings produced at lower temperatures, while Cr-rich precipitates were observed in the inner regions of coatings produced at 1000 °C. These observations indicate that coating development involves not only Fe–Al interdiffusion but also local changes in the distribution of alloying elements.
- The empirical regression models provided good descriptions of the relationships between processing parameters and both total coating thickness (R² = 0.981, adjusted R² = 0.949) and mass gain (R² = 0.978, adjusted R² = 0.971). The consistent trends obtained for both parameters support the interpretation of enhanced coating growth at elevated temperatures. However, these models are applicable only within the investigated temperature range of 700–1000 °C and treatment times of 1–6 h.
- Nanoindentation measurements demonstrated that the aluminide coatings exhibited substantially higher hardness than the ferritic steel substrate, with typical values of approximately 11 GPa compared with 4–5 GPa. Localized regions with hardness reaching approximately 19 GPa were also observed, potentially associated with Cr- and Si-rich precipitates. Coatings produced at 1000 °C exhibited a more gradual transition in mechanical properties towards the substrate, consistent with the development of an extended diffusion zone.
Overall, the results demonstrate that controlling the slurry aluminizing parameters enables substantial modification of coating thickness, phase constitution, chemical gradients, and local mechanical properties. The combined microstructural, chemical, crystallographic, and mechanical characterization provides a basis for further optimization of diffusion aluminide coatings on ferritic stainless steels. The formation of Fe–Al intermetallic phases suggests that these coatings have potential for protecting chromium-containing steels exposed to elevated temperatures in both oxidizing and reducing atmospheres. Further research will focus on evaluating the resistance and stability of these coatings under such exposure conditions.
Author Contributions
Conceptualization, A.K., P.K. and K.W.; methodology, A.K., P.K., K.W. and J.L.; software, A.K., P.K., K.W. and J.L.; validation, A.K., P.K., K.W. and J.L.; formal analysis, A.K.; investigation, A.K., P.K., K.W. and J.L.; resources, A.K.; data curation, A.K., P.K., K.W. and J.L.; writing—original draft preparation, A.K. and K.W.; writing—review and editing, A.K., P.K., K.W. and J.L.; visualization, A.K. and K.W.; supervision, A.K.; project administration, A.K.; funding acquisition, A.K.
Funding
This research was funded by Minister of Science and Higher Education of the Republic of Poland under the “Regional Initiative of Excellence” (RID) Programme, agreement No. RID/SP/0054/2024/01. The project is being implemented in the period 2024–2027.
Data Availability Statement
Data will be made available on request.
Acknowledgments
The authors gratefully would like to thank Dr. Josef Šepitka (formerly at Czech Technical University in Prague) for carrying out the nanoindentation measurements. His expertise and support were essential to obtaining the results. His contribution was essential to this study.
Conflicts of Interest
The authors declare no conflicts of interest.
References
- N’Dah, E.; Tsipas, S.; Hierro, M.P.; Pérez, F.J. Study of the Cyclic Oxidation Resistance of Al Coated Ferritic Steels with 9 and 12%Cr. Corros. Sci. 2007, 49, 3850–3865. [Google Scholar] [CrossRef]
- Vossen, J.P.T.; Gawenda, P.; Rahts, K.; Röhrig, M.; Schorr, M.; Schütze, M. Limits of the Oxidation Resistance of Several Heat-Resistant Steels under Isothermal and Cyclic Oxidation as Well as under Creep in Air at 650°C. Mater. At. High Temp. 1997, 14, 387–401. [Google Scholar] [CrossRef]
- Chou, Y.S.; Stevenson, J.W.; Singh, P. Effect of Aluminizing of Cr-Containing Ferritic Alloys on the Seal Strength of a Novel High-Temperature Solid Oxide Fuel Cell Sealing Glass. J. Power Sources 2008, 185, 1001–1008. [Google Scholar] [CrossRef]
- Sánchez, L.; Bolívar, F.J.; Hierro, M.P.; Trilleros, J.A.; Pérez, F.J. Effects of Reactive Gaseous Mixture and Time on the Growth Rate and Composition of Aluminium Diffusion Coatings by CVD-FBR on 12Cr-Ferritic Steel. Surf. Coat. Technol. 2007, 201, 7626–7634. [Google Scholar] [CrossRef]
- Xiang, Z.D.; Datta, P.K. Pack Aluminisation of Low Alloy Steels at Temperatures below 700 °C. Surf. Coat. Technol. 2004, 184, 108–115. [Google Scholar] [CrossRef]
- Mao, S.W.; Huang, H.L.; Gan, D. Microstructure of Aluminized Stainless Steel 310 after Annealing. Surf. Coat. Technol. 2010, 205, 533–539. [Google Scholar] [CrossRef]
- Grabke, H.J. Oxidation of NiAl and FeAl. Intermetallics 1999, 7, 1153–1158. [Google Scholar] [CrossRef]
- Tsai, W.-T.; Huang, K.-E. Microstructural Aspect and Oxidation Resistance of an Aluminide Coating on 310 Stainless Steel. Thin Solid Films 2000, 366, 164–168. [Google Scholar] [CrossRef]
- Hindam, H.; Whittle, D.P. Microstructure, Adhesion and Growth Kinetics of Protective Scales on Metals and Alloys. Oxid. Met. 1982, 18, 245–284. [Google Scholar] [CrossRef]
- Baranda, M.; Mayo, C.; Diaz, R.; Rodriguez, R.; Pérez, F.J. Comparative Environmental Assessment of Coated Ferritic Steels Suited to Steam Turbines of Coal-Fired Supercritical and Ultra-Supercritical Power Plants. J. Clean. Prod. 2024, 443, 141226. [Google Scholar] [CrossRef]
- Agüero, A.; Muelas, R.; Gutiérrez, M.; Van Vulpen, R.; Osgerby, S.; Banks, J.P. Cyclic Oxidation and Mechanical Behaviour of Slurry Aluminide Coatings for Steam Turbine Components. Surf. Coat. Technol. 2007, 201, 6253–6260. [Google Scholar] [CrossRef]
- Agüero, A.; Gutiérrez, M.; González, V. Deposition Process of Slurry Iron Aluminide Coatings. Mater. At. High Temp. 2008, 25, 257–265. [Google Scholar] [CrossRef]
- Marulanda, J.L.; Castañeda, S.I.; Pérez, F.J. Improvement in Resistance to Steam Oxidation of Aluminide-Coated AISI 304 and AISI 316 Steel Produced by Chemical Vapor Deposition in a Fluidized Bed Reactor. Oxid. Met. 2015, 84, 429–445. [Google Scholar] [CrossRef]
- Sánchez, L.; Bolívar, F.J.; Hierro, M.P.; Pérez, F.J. Temperature Dependence of the Oxide Growth on Aluminized 9-12%Cr Ferritic-Martensitic Steels Exposed to Water Vapour Oxidation. Thin Solid Films 2009, 517, 3292–3298. [Google Scholar] [CrossRef]
- Sánchez, L.; Bolívar, F.J.; Hierro, M.P.; Pérez, F.J. Behaviour of Aluminide Diffusion Coatings on HCM12-A Steel by Al/Ce and Al/La CVD-FBR in Oxidation. Defect Diffus. Forum 2009, 289–292, 461–468. [Google Scholar] [CrossRef]
- Tsai, W.-T.; Huang, K.-E. Microstructural Aspect and Oxidation Resistance of an Aluminide Coating on 310 Stainless Steel.
- Agüero, A.; González, V.; Gutiérrez, M. Long Term Diffusion Studies in Fe Aluminide Coatings Deposited by Slurry Application on Ferritic Steel. Defect Diffus. Forum 2009, 289–292, 243–251. [Google Scholar] [CrossRef]
- Chiang, K.T.; Kallenborn, K.J.; Yuen, J.L. Aluminization of Copper for Oxidation Protection. Surf. Coat. Technol. 1992, 52, 135–139. [Google Scholar] [CrossRef]
- Pint, B.A.; Zhang, Y.; Tortorelli, P.F.; Haynes, J.A.; Wright, I.G. Evaluation of Iron-Aluminide CVD Coatings for High Temperature Corrosion Protection. Mater. At. High Temp. 2001, 18, 185–192. [Google Scholar] [CrossRef]
- Zhang, Y.; Pint, B.A.; Cooley, K.M.; Haynes, J.A. Formation of Aluminide Coatings on Fe-Based Alloys by Chemical Vapor Deposition. Surf. Coat. Technol. 2008, 202, 3839–3849. [Google Scholar] [CrossRef]
- Boulesteix, C.; Pedraza, F. Characterisation of Aluminium Diffusion Coatings Elaborated on Austenitic Stainless Steels and on Ferritic-Martensitic Steels. Surf. Coat. Technol. 2018, 339, 27–36. [Google Scholar] [CrossRef]
- Hu, T.L.; Huang, H.L.; Gan, D.; Lee, T.Y. The Microstructure of Aluminized Type 310 Stainless Steel. Surf. Coat. Technol. 2006, 201, 3502–3509. [Google Scholar] [CrossRef]
- Lu, J.; Huang, J.; Wang, J.; Yang, Z.; Gu, Y. Long-Term Degradation Behavior of Slurry Aluminide Coating on Super304H Stainless Steel at 650 °C. Corros. Sci. 2021, 178, 109054. [Google Scholar] [CrossRef]
- Grabke, H.J. Oxidation of NiAl and FeAl.
- Agüero, A.; Spiradek, K.; Höfinger, S.; Gutiérrez, M.; Muelas, R. Microstructural Evolution of Slurry Fe Aluminide Coatings during High Temperature Steam Oxidation. Mater. Sci. Forum 2008, 595–598, 251–259. [Google Scholar] [CrossRef]
- Zhang, Y.; Pint, B.A.; Cooley, K.M.; Haynes, J.A. Effect of Nitrogen on the Formation and Oxidation Behavior of Iron Aluminide Coatings. Surf. Coat. Technol. 2005, 200, 1231–1235. [Google Scholar] [CrossRef]
- Li, C.; Huang, T.; Song, P.; Yuan, X.; Feng, J.; Lü, K.; Li, Q.; Duan, W.; Lu, J. Effect of Water Vapour on Morphology of the Si/Ti-Rich Phase at the Interface between Oxide Layer and Aluminide Coating. Corros. Sci. 2020, 163, 108240. [Google Scholar] [CrossRef]
- Agüero, A.; González, V.; Muelas, R. Diffusion Stable Aluminide Coatings: Behaviour under Steam and Oxy-Fuel Fire-Side Conditions at 650 °C and Accelerated Diffusion Tests at 900 °C. Surf. Coat. Technol. 2018, 350, 119–127. [Google Scholar] [CrossRef]
- Karimzadeh, A.; Rouhaghdam, A.S. Effect of Nickel Pre-Plated on Microstructure and Oxidation Behavior of Aluminized AISI 316 Stainless Steel. Mater. Manuf. Process. 2016, 31, 87–94. [Google Scholar] [CrossRef]
- Wang, Y.; Wang, J.; Hu, H.; Meng, J.; Zhao, X. Fabrication and Oxidation of an Y2O3-Modified Low Temperature Aluminide Coating on 309 Stainless Steel. Vacuum 2018, 155, 193–198. [Google Scholar] [CrossRef]
- Yener, T.; Doleker, K.M.; Erdogan, A.; Oge, M.; Er, Y.; Karaoglanli, A.C.; Zeytin, S. Wear and Oxidation Performances of Low Temperature Aluminized IN600. Surf. Coat. Technol. 2022, 436. [Google Scholar] [CrossRef]
- Khan, A.; Rauf, A.; Ullah, S.; Jan, H.U.; Aziz, T.; Zhang, S.H.; Song, G.S. ZrO2-Nanoparticle Assisted Phase Transformation and Oxidation Kinetics of Thermally Grown Alumina on Nickel Aluminide Coatings. Surf. Coat. Technol. 2023, 470. [Google Scholar] [CrossRef]
- Ebrahimifar, H.; Zandrahimi, M. Mn Coating on AISI 430 Ferritic Stainless Steel by Pack Cementation Method for SOFC Interconnect Applications. Solid State Ion. 2011, 183, 71–79. [Google Scholar] [CrossRef]
- Azadi, M.; Farrahi, G.H.; Winter, G.; Eichlseder, W. Experimental Fatigue Lifetime of Coated and Uncoated Aluminum Alloy under Isothermal and Thermo-Mechanical Loadings. Ceram. Int. 2013, 39, 9099–9107. [Google Scholar] [CrossRef]
- Hintsala, E.D.; Hangen, U.; Stauffer, D.D. High-Throughput Nanoindentation for Statistical and Spatial Property Determination. JOM 2018, 70, 494–503. [Google Scholar] [CrossRef]
- Shabanov, Y.; Zhumagaliyev, Y.; Nurgali, N.; Dossekenov, M.; Almuratova, K.; Orynbassar, R.; Kainenova, T.; Bakirova, B.; Kanapiyeva, F.; Zhunussova, E. Exploring Alloy Composition Dynamics: Thermodynamic Analysis of Fe-Al-Si-Cr System in Homogeneous Liquid State. Processes 2024, 12, 1947. [Google Scholar] [CrossRef]
- Jiang, S.; Ding, H.; Xu, J. Cavitation Erosion Resistance of Sputter-Deposited Cr3Si Film on Stainless Steel. J. Tribol. 2017, 139. [Google Scholar] [CrossRef]
- Zou, C.W.; Wang, H.J.; Feng, L.; Xue, S.W. Effects of Cr Concentrations on the Microstructure, Hardness, and Temperature-Dependent Tribological Properties of Cr-DLC Coatings. Appl. Surf. Sci. 2013, 286, 137–141. [Google Scholar] [CrossRef]
- Qiu, J.; Li, Y.; Luo, X.; Zhou, H.; Cao, C.; Bi, G. Silicon Regulation of the Interface Microstructure and Shear Strength of Rheological Cast-Rolling Aluminum/Steel Composite Plates. J. Mater. Res. Technol. 2024, 30, 6812–6828. [Google Scholar] [CrossRef]
- Yu, X.; Huang, J.; Yang, T.; Fan, D. The Growth Behavior for Intermetallic Compounds at the Interface of Aluminum-Steel Weld Joint. Materials 2022, 15, 3563. [Google Scholar] [CrossRef] [PubMed]
- Wang, H.; Sun, S.; Li, X.; Wang, J.; Su, X. Effect of Silicon on Interfacial Reaction and Morphology of Hot-Dip Aluminizing. J. Mater. Res. Technol. 2022, 20, 3723–3734. [Google Scholar] [CrossRef]
- ZOU, T.; YU, G.; CHEN, S.; HUANG, J.; YANG, J.; ZHAO, Z.; RONG, J.; YANG, J. Effect of Si Content on Interfacial Reaction and Properties between Solid Steel and Liquid Aluminum. Trans. Nonferrous Met. Soc. China 2021, 31, 2570–2584. [Google Scholar] [CrossRef]
- Sakidja, R.; Perepezko, J.H.; Calhoun, P. Synthesis, Thermodynamic Stability and Diffusion Mechanism of Al 5 Fe 2-Based Coatings. [CrossRef]
Figure 2.
Mass changes after the slurry aluminizing process.

Figure 3.
The microstructure (BEI) of coatings obtained: at 700°C for (a) 1 hour - No. 1, (b) 2 hours - No. 2, (c) 6 hours - No. 3; at 800°C for (d) 1 hour - No. 4, (e) 2 hours - No. 5, (f) 6 hours - No. 6; at 1000°C for (g) 1 hour - No. 7, (h) 2 hours - No. 8, (i) 6 hours - No. 9.
Figure 3.
The microstructure (BEI) of coatings obtained: at 700°C for (a) 1 hour - No. 1, (b) 2 hours - No. 2, (c) 6 hours - No. 3; at 800°C for (d) 1 hour - No. 4, (e) 2 hours - No. 5, (f) 6 hours - No. 6; at 1000°C for (g) 1 hour - No. 7, (h) 2 hours - No. 8, (i) 6 hours - No. 9.

Figure 4.
Thickness of Si-Al coatings obtained for different manufacturing parameters.

Figure 5.
a) Thickness of Si-Al coatings obtained for different manufacturing parameters; b) mass changes after the slurry aluminizing process depending on different manufacturing parameters.
Figure 5.
a) Thickness of Si-Al coatings obtained for different manufacturing parameters; b) mass changes after the slurry aluminizing process depending on different manufacturing parameters.

Figure 6.
Elemental mapping in cross section in Al-Si coating a) No 1 (manufactured at 700°C, 1 h); b) No 4 (manufactured at 800°C, 1 h); c) No 7 (manufactured at 1000°C, 1 h).
Figure 6.
Elemental mapping in cross section in Al-Si coating a) No 1 (manufactured at 700°C, 1 h); b) No 4 (manufactured at 800°C, 1 h); c) No 7 (manufactured at 1000°C, 1 h).

Figure 7.
Line and point analysis (EDS) in cross section in coating a) No 2 (manufactured at 700°C, 2 h); b) No 5 (manufactured at 800°C, 2 h); c) No 8 (manufactured at 1000°C, 2 h).
Figure 7.
Line and point analysis (EDS) in cross section in coating a) No 2 (manufactured at 700°C, 2 h); b) No 5 (manufactured at 800°C, 2 h); c) No 8 (manufactured at 1000°C, 2 h).

Figure 8.
COMPASS spectral classification maps and corresponding cumulative EDS spectra of coatings produced at (a) 700 °C for 1 h and (b) 1000 °C for 2 h.
Figure 8.
COMPASS spectral classification maps and corresponding cumulative EDS spectra of coatings produced at (a) 700 °C for 1 h and (b) 1000 °C for 2 h.

Figure 9.
XRD patterns of Si-Al coating obtained on X3CrTi17 alloy.

Figure 10.
Microstructure (BEI) of a cross-section of aluminide coatings formed on X3CrTi17 steel, along with contour maps showing local hardness and elastic reduced modulus values obtained via nanoindentation.
Figure 10.
Microstructure (BEI) of a cross-section of aluminide coatings formed on X3CrTi17 steel, along with contour maps showing local hardness and elastic reduced modulus values obtained via nanoindentation.

Table 1.
Technological parameters of coatings production.
| No of sample | Annealing temperature [°C] | Annealing duration [h] |
| 1 | 700 | 1 |
| 2 | 2 | |
| 3 | 6 | |
| 4 | 800 | 1 |
| 5 | 2 | |
| 6 | 6 | |
| 7 | 1000 | 1 |
| 8 | 2 | |
| 9 | 6 |
Table 2.
The results of the EDS point analysis (at. %) indicated in Figure 7.
Table 2.
The results of the EDS point analysis (at. %) indicated in Figure 7.
| Point | EDS point analysis (at. %) | Probable phases | |||
| Al | Si | Cr | Fe | ||
| 1 | 72.3 | 0.9 | 0.6 | 26.3 | Al₅Fe₂ |
| 2 | 31.6 | 3.1 | 8.7 | 56.6 | AlFe |
| 3 | 0.3 | 1.2 | 13.1 | 85.3 | Substrate |
| 4 | 68.6 | 0.0 | 1.0 | 30.5 | Al₅Fe₂ |
| 5 | 64.5 | 0.1 | 2.9 | 32.6 | Al₅Fe₂ |
| 6 | 28.1 | 16.0 | 44.5 | 11.4 | Cr₃Si |
| 7 | 47.7 | 0.7 | 6.1 | 45.5 | AlFe |
| 8 | 1.4 | 0.8 | 41.1 | 56.7 | Substrate |
| 9 | 44.6 | 0.8 | 6.5 | 48.2 | AlFe |
| 10 | 25.1 | 1.2 | 11.0 | 62.7 | Fe-Al-Cr solid solution |
| 11 | 15.2 | 1.3 | 16.5 | 67.0 | Fe-Cr-Al solid solution |
| 12 | 0.2 | 1.1 | 15.0 | 83.7 | Substrate |
Table 3.
Average content of chemical elements in phases according to Figure 8.
Table 3.
Average content of chemical elements in phases according to Figure 8.
| Element | EDS analysis (at. %) | |||||||
| Phase 1 | Phase 2 | Phase 3 | Phase 4 | Phase 5 | Phase 6 | Phase 7 | Phase 8 | |
| Al | 66.0 | 2.0 | 41.1 | 33.2 | 64.6 | 10.4 | 37.9 | 4.0 |
| Si | 2.9 | 1.4 | 21.4 | 9.1 | 10.4 | 1.6 | 1.1 | 0.9 |
| Cr | 2.4 | 13.6 | 6.0 | 25.8 | 5.1 | 11.8 | 7.7 | 49.6 |
| Fe | 28.7 | 83.0 | 31.5 | 31.8 | 19.9 | 76.2 | 53.3 | 45.5 |
| Probable phases or chemically distinct regions | Al₅Fe₂-type | Fe-Cr solid solution | Al-Fe-Si-rich phase | Cr₃Si-type precipitates | Si-containing Al₅Fe₂-type | Al-containing Fe-Cr solid solution | AlFe | Cr-rich precipitates (possible chromium carbides) |
Disclaimer/Publisher’s Note: The statements, opinions and data contained in all publications are solely those of the individual author(s) and contributor(s) and not of MDPI and/or the editor(s). MDPI and/or the editor(s) disclaim responsibility for any injury to people or property resulting from any ideas, methods, instructions or products referred to in the content. |
© 2026 by the authors. Licensee MDPI, Basel, Switzerland. This article is an open access article distributed under the terms and conditions of the Creative Commons Attribution (CC BY) license (http://creativecommons.org/licenses/by/4.0/).